Etherification reaction catalyst and preparation method thereof and process for preparing ethylene glycol tert-butyl ether
By using a modified acidic resin and a mixture of amorphous silica and aluminum catalysts, the problems of high isobutylene content and numerous byproducts in the preparation of ethylene glycol monotert-butyl ether were solved, improving product selectivity, reducing energy consumption, and simplifying the separation process.
Patent Information
- Application Number
- CN202111280149.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-29
AI Technical Summary
Existing technologies for preparing ethylene glycol monotert-butyl ethers require high isobutylene content and have an excessively high proportion of byproducts, resulting in low product selectivity, complex separation processes, and high energy consumption.
A mixture of modified acid resin and amorphous silica-alumina was used as the catalyst for the etherification reaction. The acid resin was modified by heat treatment and calcination, and then reacted with ethylene glycol and isobutylene under etherification reaction conditions. The reaction conditions were optimized to reduce the isobutylene content and the formation of byproducts.
The minimum content requirement of isobutylene in the reaction feedstock was lowered, the selectivity of ethylene glycol monotert-butyl ether was improved, the amount of by-products generated was reduced, the product separation steps were simplified, and energy consumption was reduced.
Smart Images

Figure CN116060128B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of petrochemical industry, and in particular, to an etherification reaction catalyst and a preparation method thereof, as well as a process for preparing ethylene glycol tert-butyl ether. Background Art
[0002] Ethylene glycol mono-tert-butyl ether (ETB) has the advantages of high volatility, low odor, low toxicity, low photochemical reactivity, etc. It is mild to skin irritation, has good solubility in water, has good dispersion stability in latex coatings, and is soluble in most resins and organic solvents. It can be widely used in coatings, inks, dyes, cleaning agents, rust removers, brake fluids, cutting fluids, electronic strippers, fiber wetting agents, plasticizers, organic synthesis intermediates, paint strippers and other fields.
[0003] ETB is an environmentally friendly alcohol ether solvent that can replace EB, which pollutes the environment. The main preparation technologies currently include Maruzen Technology of Japan, Sinopec Shanghai Institute Technology, Shandong Wanhua Technology, Shenzhen Feiyang Technology, etc. The common problems of the above technologies are: (1) LPG with an isobutylene content of 30% to 100% can be used, but LPG with an isobutylene content of less than 20% cannot be used; (2) The selectivity of ETB in the product is low; (3) The selectivity of the by-product diisobutylene is high; (4) The low selectivity of ETB in the product leads to more impurities, which in turn affects the separation process, resulting in a complex process, high investment and energy consumption; the above problems need to be solved. Summary of the invention
[0004] The purpose of the present disclosure is to solve the problems of high isobutylene content requirement, high proportion of by-products and low selectivity of ETB in the product in the prior art ethylene glycol tert-butyl ether process.
[0005] To solve the above problems, the first aspect of the present disclosure provides a method for preparing an etherification reaction catalyst, wherein the etherification reaction catalyst comprises a mixture of a modified acidic resin and amorphous silica-alumina; the method comprises the following steps of preparing the modified acidic resin: contacting an acidic ion exchange resin and an organic ester under a protective atmosphere for heat treatment, and subjecting the obtained materials to solid-liquid separation to obtain a heat-treated resin; contacting the heat-treated resin with an organic solvent, and then calcining to obtain a modified acidic resin; wherein the heat treatment temperature is 50 to 200°C.
[0006] Optionally, the organic ester is selected from fatty acid esters with carbon atoms of 2 to 5 and / or aromatic acid esters with carbon atoms of 7 to 12; the organic ester is a monobasic acid ester; preferably, the organic ester is selected from one or more of methyl formate, ethyl formate, ethyl acetate, methyl propionate, ethyl propionate, n-propyl formate, isopropyl formate, methyl methoxyacetate, ethyl methoxyacetate, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, methyl hydroxybenzoate, ethyl hydroxybenzoate and butyl hydroxybenzoate, and more preferably one or more of ethyl methoxyacetate, isopropyl formate, methyl benzoate and methyl hydroxybenzoate.
[0007] Optionally, the protective atmosphere includes one or more of nitrogen, argon, helium, carbon monoxide and carbon dioxide, preferably nitrogen.
[0008] Optionally, the organic solvent includes one or more of ethanol, n-propanol, n-butanol, isopropanol, sec-butanol and tert-butanol, preferably ethanol.
[0009] Optionally, the heat treatment pressure is 0.1-20.0 MPa, the temperature is 80-150° C., and the time is 0.2-30 h; relative to 1 g of the acidic ion exchange resin, the amount of the organic ester is 0.5-2.5 mL.
[0010] Optionally, the method includes soaking the heat-treated resin in the organic solvent, taking out the soaked resin, and then performing the calcination; the soaking temperature is 10 to 50°C and the time is 3 to 10 hours; the calcination temperature is 70 to 120°C and the time is 1 to 5 hours.
[0011] Optionally, the acidic ion exchange resin is selected from a strong acidic ion exchange resin and / or a weak acidic ion exchange resin, preferably a macroporous strong acidic ion exchange resin.
[0012] Optionally, the amorphous silicon aluminum contains 0-0.3 wt% Na2O, 50-80 wt% SiO2 and 20-50 wt% Al2O3, wherein the contents of Na2O, SiO2 and Al2O3 are measured by XRF method; in the XRD spectrum of the amorphous silicon aluminum, only one diffuse diffraction peak appears at 25°-27°, the most probable pore size of the amorphous silicon aluminum is 20-50 nm, and x / y is 0.55-0.75, wherein x represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by XPS method, and y represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by XRF method.
[0013] Optionally, the method further comprises mixing the modified acidic resin and the amorphous silica-alumina to obtain the etherification reaction catalyst.
[0014] Optionally, based on dry weight, the mass ratio of the modified acidic resin to the amorphous silica-alumina is (0.3-3):1.
[0015] Optionally, the average particle size of the modified acidic resin is 0.350-1.250 mm, and the average particle size of the amorphous silicon aluminum is 0.030-0.100 μm.
[0016] In a second aspect of the present disclosure, an etherification reaction catalyst is prepared by the method described in the first aspect of the present disclosure.
[0017] The third aspect of the present disclosure provides a process for preparing ethylene glycol mono-tert-butyl ether, which comprises: under etherification reaction conditions, contacting ethylene glycol, a C4 olefin raw material containing isobutylene and methyl tert-butyl ether in the presence of the etherification reaction catalyst described in the second aspect of the present disclosure.
[0018] Optionally, the mass fraction of isobutylene in the C4 olefin feedstock is 5 to 100%, preferably 10 to 100%; the molar ratio of the total amount of isobutylene and the methyl tert-butyl ether in the C4 olefin feedstock to the ethylene glycol is 1:1 to 10, preferably 1:2 to 4.
[0019] Optionally, the method further includes adding an additive to the contact reaction, wherein the additive is selected from water and / or alcohol, preferably one or more of water, ethanol, n-propanol, isopropanol and tert-butanol; the ratio of the weight of the additive to the total weight of the ethylene glycol and the mixed C4 olefins is 0.005 to 0.2:1, preferably 0.02 to 0.1:1.
[0020] Optionally, the etherification reaction conditions include: reaction temperature of 40 to 100°C, preferably 60 to 80°C; reaction pressure of 0.5 to 2.5 MPa, preferably 0.5 to 1.5 MPa; space velocity of 0.1 to 10 h -1 , preferably 0.3~1.0h -1 .
[0021] Optionally, the method further comprises sending the material obtained from the contact reaction into a separation unit for separation to obtain ethylene glycol mono-tert-butyl ether; the separation unit comprises a C4 removal tower, a light removal tower, a C8 removal tower, a MTBE removal tower, an azeotropic tower, an ethylene glycol flash tower and an ETB separation tower.
[0022] Through the above technical scheme, the etherification reaction catalyst obtained by the preparation method disclosed in the present invention can reduce the minimum content requirement of isobutylene in the reaction raw material C4 olefin in the preparation process of ethylene glycol mono-tert-butyl ether, can greatly reduce the amount of by-products generated, increase the selectivity for ETB, and thus reduce the energy consumption of the product separation step.
[0023] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0025] Figure 1 It is a process flow chart of a specific implementation method of the process for preparing ethylene glycol mono-tert-butyl ether disclosed in the present invention.
[0026] Description of Reference Numerals
[0027] 1. Etherification reactor; 2. C4 removal tower; 3. Light removal tower; 4. MTBE removal tower; 5. C8 removal tower; 6. Azeotropic tower; 7. ETB separation tower; 8. Ethylene glycol flash tower; 9. Heavy components; 10. Circulating EG; 11. Circulating EDB; 12. Circulating MTBE; 13. Methanol; 14. ETB product; 15. EG; 16. C4 olefin feedstock; 17. Methyl tert-butyl ether; 18. Mixed C4 materials; 19. C8 logistics. DETAILED DESCRIPTION
[0028] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0029] In the present disclosure, unless otherwise specified, "EG" refers to ethylene glycol, "C4" refers to mixed C4 olefins in the reaction feedstock, "MTBE" refers to methyl tert-butyl ether, "ETB" refers to ethylene glycol mono-tert-butyl ether, "EDB" refers to ethylene glycol di-tert-butyl ether, and "IB" refers to isobutylene. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise specified.
[0030] The first aspect of the present disclosure provides a method for preparing an etherification reaction catalyst, wherein the etherification reaction catalyst comprises a mixture of a modified acidic resin and amorphous silica-alumina; the method comprises the following steps of preparing the modified acidic resin: contacting an acidic ion exchange resin and an organic ester under a protective atmosphere for heat treatment, and subjecting the obtained material to solid-liquid separation to obtain a heat-treated resin; contacting the heat-treated resin with an organic solvent, and then calcining to obtain a modified acidic resin; wherein the heat treatment temperature is 50 to 200°C.
[0031] Through the above technical scheme, the preparation method disclosed in the present invention obtains a modified acidic resin by modifying an acidic ion exchange resin with an organic ester. The mixture of the modified acidic resin and amorphous silicon aluminum is used as an etherification reaction catalyst to prepare an etherification reaction catalyst for the preparation of ethylene glycol mono-tert-butyl ether, which can reduce the minimum content requirement of isobutylene in the reaction raw material C4 olefin from 20 weight % to 5 weight %, and at the same time, can reduce the content of isobutylene in the C4 olefin after the etherification reaction, generally can be lower than 3 weight %; can greatly reduce the amount of by-product C8 olefins, etc., generally can be lower than 5 weight %; increase the selectivity of ETB, the selectivity can be as high as 90 weight %, and thus can reduce the energy consumption of the product separation step.
[0032] In one embodiment, the method of the present disclosure further comprises subjecting the acidic ion exchange resin to heat treatment in a reactor selected from one or more of a stirred tank reactor, a trickle bed reactor and a fixed bed reactor, preferably a fixed bed reactor.
[0033] In one embodiment, the heat treatment of the acidic ion exchange resin and the organic ester under a protective atmosphere may include: pumping the organic ester into a reactor under a protective atmosphere, and then adding the acidic ion exchange resin. The amount of the organic ester may vary within a wide range, preferably, the amount of the organic ester may be 0.5 to 2.5 mL, preferably 0.5 to 1.5 mL, relative to 1 g of the acidic ion exchange resin.
[0034] In one embodiment, the organic ester is selected from fatty acid esters having 2 to 5 carbon atoms and / or aromatic acid esters having 7 to 12 carbon atoms; the organic ester is a monobasic acid ester; preferably, the organic ester is selected from one or more of methyl formate, ethyl formate, ethyl acetate, methyl propionate, ethyl propionate, n-propyl formate, isopropyl formate, methyl methoxyacetate, ethyl methoxyacetate, methyl benzoate, ethyl benzoate, butyl benzoate, methyl hydroxybenzoate, ethyl hydroxybenzoate and butyl hydroxybenzoate, and more preferably one or more of ethyl methoxyacetate, isopropyl formate, methyl benzoate, butyl benzoate and methyl hydroxybenzoate.
[0035] In this embodiment, the organic ester used is an organic substance containing an ester functional group, which can remove moisture from the resin, increase the size of the resin pores and modify the structure of the resin. The activity of the modified acidic resin can be further enhanced by selecting the preferred organic ester.
[0036] In one embodiment, the protective atmosphere is, for example, a gas atmosphere having an oxygen content of less than 1.0 volume % and a water content of less than 1.0 volume %. In a preferred embodiment, the protective atmosphere includes one or more of nitrogen, argon, helium, carbon monoxide and carbon dioxide, preferably nitrogen. In other embodiments, no specific requirements are made for the water content and oxygen content of the protective atmosphere, for example, the protective atmosphere can be derived from a commercially available protective atmosphere.
[0037] In this embodiment, the use of a protective atmosphere during the modification process can reduce the oxygen content in the acidic ion exchange resin and enhance the modification effect. After the modification is completed, the organic ester is pushed out with a protective atmosphere, and then the organic ester is swept away with a protective atmosphere to achieve the effect of solid-liquid separation.
[0038] According to the method disclosed herein, conventional methods can be used to perform solid-liquid separation to separate the heat-treated resin from the heat-treated material; in one embodiment, a protective atmosphere gas can be used for solid-liquid separation, for example, the liquid in the reaction container can be blown out by the protective atmosphere, and preferably, the protective atmosphere can then be used to further remove the liquid to obtain the heat-treated resin.
[0039] According to the present disclosure, contacting the heat-treated resin with an organic solvent may include washing or soaking the heat-treated resin with an organic solvent. The amount of the organic solvent is not particularly limited. For example, relative to 1 g of the heat-treated resin, the amount of the organic solvent may be 0.1 to 5 mL, preferably 0.5 to 2.5 mL, and more preferably 0.5 to 1.5 mL.
[0040] In one embodiment, the organic solvent comprises an alcohol, preferably a C2-C5 alcohol, for example, one or more selected from ethanol, n-propanol, n-butanol, n-pentanol, isopropanol, isobutanol, sec-butanol and tert-butanol, more preferably ethanol.
[0041] In this embodiment, by soaking the heat-treated resin in an organic solvent, the organic ester remaining in the heat-treated resin can be cleaned and the activity of the modified acidic resin can be enhanced.
[0042] In one embodiment, the heat treatment pressure is 0.1-20.0 MPa, the temperature is 80-150°C, and the time is 0.2-30 h; preferably, the heat treatment pressure is 0.1-15 MPa, the temperature is 100-130°C, and the time is 0.5-20 h.
[0043] In one embodiment, the method comprises: soaking the heat-treated resin in the organic solvent, taking out the soaked resin, and then performing the calcination; wherein the soaking temperature can be 10 to 50°C, preferably 20 to 40°C, and the time is 3 to 10 hours, preferably 3 to 5 hours; the calcination temperature can be 70 to 120°C, preferably 80 to 110°C, and the time can be 1 to 5 hours, preferably 2 to 4 hours.
[0044] In this embodiment, the calcination treatment can be performed in an oven, for example, the soaked resin is treated. The heat treatment conditions and subsequent treatment conditions can make the performance of the modified acidic resin more excellent. By optimizing the heat treatment temperature, the catalytic performance of the modified acidic resin can be further enhanced.
[0045] In one embodiment, the acidic ion exchange resin is selected from a strong acidic ion exchange resin and / or a weak acidic ion exchange resin, preferably a macroporous strong acidic ion exchange resin. In this embodiment, the modified acidic resin obtained by modifying the preferred macroporous strong acidic ion exchange resin has better catalytic performance.
[0046] In one embodiment, the amorphous silicon aluminum contains 0-0.3 wt % Na2O, 50-80 wt % SiO2 and 20-50 wt % Al2O3, wherein the contents of Na2O, SiO2 and Al2O3 are measured by XRF method; in the XRD spectrum of the amorphous silicon aluminum, only one diffuse diffraction peak appears at 25°-27°, the most probable pore size of the amorphous silicon aluminum is 20-50 nm, and x / y is 0.55-0.75, wherein x represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by XPS method, and y represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by XRF method.
[0047] In one embodiment, the method for preparing the amorphous silicon-aluminum comprises: fully mixing a silicon source and an alkali solution at room temperature to 60°C, adding an aluminum source under stirring, adjusting the resulting slurry to an endpoint pH value between 8 and 10.5, and then dynamically aging at a constant temperature of 40 to 80°C, washing, filtering, and obtaining a solid precipitate; contacting the solid precipitate with a dilute acid solution at a weight ratio of solid precipitate: acid: H2O = 1: (0.02 to 0.20): (5 to 30) at room temperature to 60°C for at least 0.2 hours, filtering, and drying at 100 to 150°C; wherein the silicon source and the aluminum source are The weight ratio is 1:(0.25-1), the silicon source is calculated as silicon oxide, and the aluminum source is calculated as aluminum oxide; the chemical composition of the amorphous silicon aluminum catalytic material measured by XRF method is: (0-0.3)Na2O·(50-80)SiO2·(20-50)Al2O3 by weight of the oxide; in the XRD spectrum of the silicon aluminum material, only one diffuse diffraction peak appears at 25°-27°, and the most probable pore size is 20-50nm; x / y=0.55-0.75, wherein x represents the Si / Al atomic ratio measured by XPS method, and y represents the Si / Al atomic ratio measured by XRF method.
[0048] In one embodiment, the modified acidic resin and amorphous silica-alumina are mixed to obtain the etherification reaction catalyst.
[0049] In one embodiment, on a dry basis, the mass ratio of the modified acidic resin to the amorphous silica-alumina is (0.3-3):1, preferably (0.5-2):1, and more preferably (0.7-1.5):1.
[0050] In one embodiment, the average particle size of the modified acidic resin is 0.350-1.250 mm, and the average particle size of the amorphous silicon aluminum is 0.030-0.100 μm.
[0051] In a second aspect of the present disclosure, an etherification reaction catalyst is prepared by the method described in the first aspect of the present disclosure.
[0052] The third aspect of the present disclosure provides a process for preparing ethylene glycol mono-tert-butyl ether, which comprises: under etherification reaction conditions, contacting ethylene glycol, a C4 olefin raw material containing isobutylene and methyl tert-butyl ether in the presence of the etherification reaction catalyst described in the second aspect of the present disclosure.
[0053] In this embodiment, the reaction is performed by loading the etherification reaction catalyst into a reactor selected from a stirred tank reactor, a trickle bed reactor and a fixed bed reactor, preferably a fixed bed reactor, and then adding the reaction materials therein for contact reaction.
[0054] According to the present disclosure, the C4 olefin raw material contains isobutylene. In a preferred embodiment, the mass fraction of isobutylene in the C4 olefin raw material is 5 to 100%, preferably 10 to 100%, so as to further improve the reaction effect of the catalytic etherification reaction.
[0055] In one embodiment, the molar ratio of the total amount of isobutylene and the methyl tert-butyl ether in the C4 olefin raw material to the ethylene glycol is 1:1-10, preferably 1:2-4. The etherification reaction conditions include: reaction temperature of 40-100°C, preferably 60-80°C; reaction pressure of 0.5-2.5MPa, preferably 0.5-1.5MPa; space velocity of 0.1-10h -1 , preferably 0.3~1.0h -1 .
[0056] In the above preferred embodiment, the alcohol-olefin molar ratio of ethylene glycol and C4 olefin raw materials and methyl tert-butyl ether and the conditions of the etherification reaction can work synergistically to further promote the complete reaction, improve the conversion rate of isobutylene and methyl tert-butyl ether and the selectivity of the product ETB, thereby improving the raw material utilization rate and reducing the energy consumption of the subsequent separation process.
[0057] In one embodiment, the method further includes adding an additive to the contact reaction, wherein the additive is selected from water and / or alcohol, preferably one or more of water, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol and tert-butanol; the ratio of the weight of the additive to the total weight of the ethylene glycol and the mixed C4 olefins, that is, the weight ratio of additive / (ethylene glycol+mixed C4 olefins) is 0.005 to 0.2:1, preferably 0.02 to 0.1:1.
[0058] In this embodiment, by adding additives, the acidity of the etherification reaction catalyst can be reduced, the catalyst activity can be adjusted, and further, the generation of by-products can be reduced, and the energy consumption of the product separation step can be reduced.
[0059] In one embodiment, the method further includes sending the material obtained from the contact reaction into a separation unit for separation to obtain ethylene glycol mono-tert-butyl ether; the separation unit includes a C4 removal tower, a light removal tower, a C8 removal tower, a MTBE removal tower, an azeotropic tower, an ethylene glycol flash tower and an ETB separation tower.
[0060] In one embodiment, if Figure 1 As shown, the materials obtained by the reaction are separated by the following steps:
[0061] Ethylene glycol 15, C4 olefin raw material 16 and methyl tert-butyl ether 17 are pumped into the etherification reactor 1 for reaction. The bottom material of the etherification reactor 1 enters the C4 removal tower 2, and the mixed C4 material 18 is discharged from the top of the C4 removal tower 2. The bottom material of the C4 removal tower 2 is introduced into the light removal tower 3, and the top material of the light removal tower 3 enters the MTBE removal tower 4. The circulating MTBE 12 discharged from the top of the MTBE removal tower 4 returns to the etherification reactor 1. Methanol 13 is discharged from the bottom of the MTBE removal tower 4 and can be used as a product delivery system. The bottom material of the light removal tower 3 is introduced into the C8 removal tower 5, and C8 logistics 19 is discharged from the top of the C8 removal tower 5. The bottom logistics of the C8 removal tower 5 enters the azeotropic tower 6, and the top logistics of the azeotropic tower 6 enters the ETB separation tower 7. The circulating EDB discharged from the top of the tower 7 11 returns to the etherification reactor 1, ETB product 14 comes out from the bottom of tower 7, the bottom material of azeotropic tower 6 enters ethylene glycol flash tower 8, circulating ethylene glycol 10 comes out from the top of ethylene glycol flash tower 8 and returns to the etherification reactor 1, and heavy component 9 comes out from the bottom of ethylene glycol flash tower 8.
[0062] The present disclosure is further described in detail by way of examples. The raw materials used in the examples can all be obtained through commercial sources.
[0063] In the following examples and comparative examples, the average particle size was measured using a Tristar 3020 fully automatic specific surface area and pore size analyzer produced by Micromeritics, USA; XRF was measured using a Shimadzu LAB CENTER XRF-1 wavelength dispersive X-ray fluorescence spectrometer; XRD was measured using a D / max-rA rotating anode X-ray diffractometer produced by Rigaku Corporation of Japan; and XPS was measured using a KratosAxis Ultra DLD multifunctional electron spectrometer.
[0064] Preparation Example 1
[0065] 50g of Amberlyst 15 acidic ion exchange resin (purchased from Tianjin Shuanglian Technology Co., Ltd.) was loaded into a fixed bed reactor, and 100mL of ethyl methoxylate was pumped into the reactor under nitrogen conditions. The acidic ion exchange resin was heated at 100°C for 10.0h under 5.0MPa conditions, and then the ethyl methoxylate solution was pushed out with nitrogen, and then the solvent was purged with nitrogen to obtain a heat-treated resin. The heat-treated resin was placed in a stoppered conical flask, and 200mL of ethanol was added to soak for 10h, and the ethanol was poured out. The wet resin was calcined in an oven at 105°C for 3h to obtain a modified acidic resin with an average particle size of 0.6mm.
[0066] After fully mixing a water glass solution (80 wt% SiO2 / L) and a quantitative sodium hydroxide solution with a concentration of 1.0 M at room temperature to 60°C, Al2(SO4)3 solution is added under stirring, and the pH value of the resulting slurry is adjusted to between 8 and 10.5, and then dynamically aged at a constant temperature of 40 to 80°C, washed, and filtered to obtain a solid precipitate; the solid precipitate and a dilute acid solution are mixed at a weight ratio of solid precipitate: acid: H2O = 1:0.15:15 at room temperature to 6 The mixture was contacted at 0°C for at least 0.2 hours, filtered and dried at 150°C to obtain amorphous silicon aluminum. XRF method showed that the amorphous silicon aluminum contained 0.3 wt% Na2O, 60 wt% SiO2 and 39.7 wt% Al2O3. In the XRD spectrum, only a diffuse diffraction peak appeared at 25°~27°, the most probable pore size was 43 nm, the Si / Al atomic ratio x / y measured by XPS method was 0.65, and the average particle size was 0.050 μm.
[0067] The modified acidic resin and the amorphous silicon-alumina were uniformly mixed in a mass ratio of 1.5:1 to obtain an etherification reaction catalyst Z1.
[0068] Preparation Example 2
[0069] The preparation method of the etherification reaction catalyst Z2 is the same as that of Preparation Example 1, except that the heat treatment temperature during the preparation of the modified acidic resin is 180°C.
[0070] Preparation Example 3
[0071] The preparation method of etherification reaction catalyst Z3 is the same as that of Preparation Example 1, except that ethyl methoxyacetate is replaced by an equal volume of butyl benzoate, the heat treatment temperature is 110°C, and the pressure is 8 MPa; the heat-treated resin is immersed in ethanol at 40°C for 3h, and the calcination temperature is 110°C.
[0072] Preparation Example 4
[0073] The preparation method of the etherification reaction catalyst Z4 is the same as that of Preparation Example 1, except that the mass ratio of the modified acidic resin to the amorphous silica-alumina is 2.5:1.
[0074] Preparation Example 5
[0075] The preparation method of etherification reaction catalyst Z5 is the same as that of Preparation Example 1, except that the average particle size of the prepared amorphous silicon aluminum is 0.10 μm.
[0076] Preparation Comparative Example 1
[0077] The preparation method of etherification reaction catalyst DZ1 is the same as that of Preparation Example 1, except that the heat treatment temperature during the preparation of the modified acidic resin is 40°C.
[0078] Preparation Comparative Example 2
[0079] The preparation method of etherification reaction catalyst DZ2 is the same as that of Preparation Example 1, except that ethyl methoxyacetate is not added during the heat treatment.
[0080] Preparation Comparative Example 3
[0081] The preparation method of etherification reaction catalyst DZ3 is the same as that of Preparation Example 1, except that no protective gas is used.
[0082] Preparation Comparative Example 4
[0083] The preparation method of the etherification reaction catalyst DZ4 is the same as that of Preparation Example 1, except that the etherification reaction catalyst does not contain amorphous silicon aluminum.
[0084] Preparation Comparative Example 5
[0085] The preparation method of the etherification reaction catalyst DZ5 is the same as that of Preparation Example 1, except that the etherification reaction catalyst does not contain modified acidic resin.
[0086] Example 1
[0087] 20.0 g of catalyst Z1 was filled in a fixed bed reactor on a high pressure microreactor test device. Test conditions: 0.20 ml / min (12 g / h) of ethylene glycol feed, 0.004 ml / min (0.24 g / h) of water feed, 0.060 ml / min (3.6 g / h) of C4 olefin feed with a mass fraction of isobutylene of 50%, and 0.055 ml / min (2.5 g / h) of MTBE were added to the 20 mL fixed bed reactor; the molar ratio of ene alcohol was 1:3, the reaction temperature was 70°C, the reaction pressure was 1.5 MPa, and the space velocity was 1.0 h -1 The mixed material obtained from the fixed bed reactor enters the C4 removal tower, the light removal tower, the C8 removal tower, the MTBE removal tower, the azeotropic tower, the ethylene glycol flash tower and the ETB separation tower for separation in sequence, and the ethylene glycol mono-tert-butyl ether product is obtained from the ethylene glycol mono-tert-butyl ether tower. The product properties are listed in Table 1. The olefin molar ratio refers to the molar ratio of the total amount of isobutylene and methyl tert-butyl ether in the C4 olefin raw material to ethylene glycol.
[0088] Example 2
[0089] The process for preparing ETB is the same as that in Example 1, except that the additive is isopropanol, the ethylene glycol feed rate is 0.25 ml / min (15.0 g / h), the enolate molar ratio is 1:4, the reaction temperature is 80° C., and the reaction pressure is 1.0 MPa.
[0090] Example 3
[0091] The process for preparing ETB is the same as that in Example 1, except that the mass fraction of isobutylene in the C4 olefin is 5%. The feed rate of the C4 olefin raw material with a mass fraction of isobutylene of 5% is 0.60 ml / min (36 g / h).
[0092] Example 4
[0093] The process for preparing ETB is the same as that in Example 1, except that no additive water is added.
[0094] Embodiment 5-6
[0095] The process for preparing ETB is the same as that of Example 1, except that the catalyst Z1 is replaced by equivalent amounts of catalysts Z2 and Z3, respectively.
[0096] Embodiment 7-8
[0097] The process for preparing ETB is the same as that of Example 1, except that the catalyst Z1 is replaced by equivalent amounts of catalysts Z4 and Z5, respectively.
[0098] Comparative Examples 1 to 6
[0099] The process for preparing ETB is the same as that of Example 1, except that the catalyst Z1 is replaced by equivalent amounts of catalysts DZ1, DZ1, DZ3, DZ4, DZ5 and unmodified Amberlyst 15 acidic ion exchange resin.
[0100] Comparative Example 7
[0101] The process for preparing ETB is the same as that in Example 1, except that MTBE is not added during the preparation process.
[0102] Test Case
[0103] The IB conversion, ETB selectivity, EDB selectivity and isobutylene dimer selectivity were calculated by the following formulas:
[0104] The conversion rate of IB can be accurately determined based on the changes in the amounts of n-butane, isobutane, cis-butene, trans-butene, isobutene and n-butene in the mixed C4.
[0105] IB conversion rate = (1-m IB / m IB0 )×100%, where m IB represents the residual mass of IB in mixed C4, m IB0 Represents the mass of the starting IB in the mixed C4.
[0106] Selectivity of ETB = m ETB / (m ETB +m EDB )×100%;
[0107] Selectivity of EDB = m EDB / (m ETB +m EDB )×100%;
[0108] Among them, m ETB Indicates the mass of ETB, m EDB Indicates the quality of EDB.
[0109] Selectivity of isobutylene dimer = m DIB / (m DIB +m IB )×100%. Among them, m DIB Indicates the mass of isobutylene dimer.
[0110] See Table 1 for detailed data.
[0111] Table 1
[0112]
[0113]
[0114] According to the data analysis in Table 1, it can be seen from the data of Examples 1 to 8 and Comparative Examples 1 to 7 that the use of the modified acidic resin prepared by the present invention for etherification reaction can enhance the IB conversion rate and the selectivity of ETB, and reduce the selectivity of EDB and the selectivity of isobutylene dimer; the data of Example 3 show that when the mass fraction of isobutylene in the reaction raw material C4 olefin is as low as 5%, the etherification reaction effect of the modified acidic resin of the present application is also good; the comparison of the data of Example 1 with that of Example 4 shows that in the preferred embodiment of the present application in which additives are added during the etherification reaction, the content of reaction by-products can be further reduced; the comparison of the data of Example 1 with that of Example 5 shows that in the preferred heat treatment temperature range of 100 to 130° C. in the present application, the etherification reaction effect is better. By comparing the data in Example 1 and Examples 7-8, it can be seen that in the embodiment in which the preferred etherification reaction catalyst of the present invention contains amorphous silica-alumina, and the mass ratio of the modified acidic resin to the amorphous silica-alumina is (0.3 to 3): 1. The average particle size of the modified acidic resin is 0.350 to 1.250 mm, and the average particle size of the amorphous silica-alumina is 0.030 to 0.100 μm, the reaction effect of the etherification reaction can be better.
[0115] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0116] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0117] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for preparing an etherification reaction catalyst, characterized in that: The etherification reaction catalyst comprises a mixture of modified acidic resin and amorphous silica-alumina; The method comprises the following steps of preparing the modified acidic resin: The acidic ion exchange resin and the organic ester are contacted with each other under a protective atmosphere for heat treatment, and the obtained material is subjected to solid-liquid separation to obtain a heat-treated resin; The heat-treated resin is contacted with an organic solvent and then calcined to obtain a modified acidic resin; wherein the heat treatment temperature is 50 to 200° C.; The organic ester is selected from fatty acid esters having 2 to 5 carbon atoms and / or aromatic acid esters having 7 to 12 carbon atoms; The calcination temperature is 70-120°C; The amorphous silicon aluminum comprises 0-0.3 wt % Na2O, 50-80 wt % SiO2 and 20-50 wt % Al2O3, wherein the contents of Na2O, SiO2 and Al2O3 are measured by XRF method; In the XRD spectrum of the amorphous silicon aluminum, only a diffuse diffraction peak appears at 25°~27°, the most probable pore size of the amorphous silicon aluminum is 20~50nm, and x / y is 0.55~0.75, wherein x represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by the XPS method, and y represents the Si / Al atomic ratio of the amorphous silicon aluminum measured by the XRF method.
2. The method according to claim 1, characterized in that The organic ester is a monobasic acid ester.
3. The method according to claim 2, characterized in that The organic ester is selected from one or more of methyl formate, ethyl formate, ethyl acetate, methyl propionate, ethyl propionate, n-propyl formate, isopropyl formate, methyl methoxyacetate, ethyl methoxyacetate, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, methyl hydroxybenzoate, ethyl hydroxybenzoate, propyl hydroxybenzoate and butyl hydroxybenzoate.
4. The method according to claim 3, characterized in that The organic ester is selected from one or more of ethyl methoxyacetate, isopropyl formate, methyl benzoate, butyl benzoate and methyl hydroxybenzoate.
5. The method according to claim 1, characterized in that The protective atmosphere includes one or more of nitrogen, argon, helium, carbon monoxide and carbon dioxide.
6. The method according to claim 5, characterized in that The protective atmosphere includes nitrogen.
7. The method according to claim 1, characterized in that The organic solvent includes one or more of ethanol, n-propanol, n-butanol, isopropanol, isobutanol, sec-butanol and tert-butanol.
8. The method according to claim 7, characterized in that The organic solvent includes ethanol.
9. The method according to claim 1, characterized in that: The heat treatment pressure is 0.1-20.0 MPa, the temperature is 80-150° C., and the time is 0.2-30 h; relative to 1 g of the acidic ion exchange resin, the amount of the organic ester is 0.5-2.5 mL.
10. The method according to claim 1, characterized in that The method comprises: soaking the heat-treated resin in the organic solvent, taking out the soaked resin, and then calcining; the soaking temperature is 10-50°C, the time is 3-10 hours; the calcining time is 1-5 hours.
11. The method according to claim 1, characterized in that: The acidic ion exchange resin is selected from a strongly acidic ion exchange resin and / or a weakly acidic ion exchange resin.
12. The method according to claim 11, characterized in that The acidic ion exchange resin is selected from macroporous strongly acidic ion exchange resin.
13. The method according to claim 1, characterized in that The method further comprises mixing the modified acidic resin and the amorphous silica-alumina to obtain the etherification reaction catalyst.
14. The method according to claim 1, characterized in that Calculated on a dry basis, the mass ratio of the modified acidic resin to the amorphous silica-alumina is (0.3-3):
1.
15. The method according to claim 1, characterized in that The average particle size of the modified acidic resin is 0.350-1.250 mm, and the average particle size of the amorphous silicon aluminum is 0.030-0.100 μm.
16. An etherification reaction catalyst prepared by the method according to any one of claims 1 to 15.
17. A process for preparing ethylene glycol mono-tert-butyl ether, characterized in that: The process comprises: under etherification reaction conditions, contacting and reacting ethylene glycol, a C4 olefin raw material containing isobutylene and methyl tert-butyl ether in the presence of the etherification reaction catalyst described in claim 16.
18. The process according to claim 17, characterized in that The mass fraction of isobutylene in the C4 olefin raw material is 5 to 100%; The molar ratio of the total amount of isobutylene and the methyl tert-butyl ether in the C4 olefin raw material to the ethylene glycol is 1:1-10.
19. The process according to claim 18, characterized in that The mass fraction of isobutylene in the C4 olefin raw material is 10-100%.
20. The process according to claim 18, characterized in that The molar ratio of the total amount of isobutylene and the methyl tert-butyl ether in the C4 olefin raw material to the ethylene glycol is 1:2-4.
21. The process according to claim 17, characterized in that The method also includes adding an additive to the contact reaction, wherein the additive is selected from water and / or alcohol; the ratio of the weight of the additive to the total weight of the ethylene glycol and the mixed C4 olefins is 0.005 to 0.2:
1.
22. The process according to claim 21, characterized in that The additive is selected from one or more of water, ethanol, n-propanol, isopropanol and tert-butanol.
23. The process according to claim 21, characterized in that The weight ratio of the additive to the total weight of the ethylene glycol and the mixed C4 olefins is 0.02 to 0.1:
1.
24. The process according to claim 17, characterized in that The etherification reaction conditions include: reaction temperature of 40-100°C, reaction pressure of 0.5-2.5 MPa, space velocity of 0.1-10 h -1 .
25. The process according to claim 24, characterized in that The reaction temperature is 60-80°C.
26. The process according to claim 24, characterized in that The reaction pressure is 0.5~1.5MPa.
27. The process according to claim 24, characterized in that Airspeed: 0.3~1.0h -1 .
28. The process of claim 17, wherein: The method also includes sending the material obtained from the contact reaction into a separation unit for separation to obtain ethylene glycol mono-tert-butyl ether; the separation unit includes a C4 removal tower, a light removal tower, a C8 removal tower, a MTBE removal tower, an azeotropic tower, an ethylene glycol flash tower and an ETB separation tower.