Modified ZSM-5 molecular sieve and its preparation method and application
Through the pore expansion treatment and silanization modification of ZSM-5 molecular sieve, the problem of external surface acidity affecting catalytic performance is solved, the liquid yield and catalyst stability of Fischer-Tropsch synthetic wax are improved, and the process is simplified.
Patent Information
- Application Number
- CN202111269787.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-10-29
AI Technical Summary
When the existing ZSM-5 molecular sieve is catalyzed with Fischer Tropsch synthetic wax hydrocracking to produce linear alkyl benzene raw materials, the acidity of the outer surface leads to side reactions, affecting the catalytic performance. The traditional silanization method is inefficient and cumbersome, and it is difficult to effectively eliminate non-information. The acid center of the zigzag pore.
Through the steps of reaming treatment, pore protection liquid impregnation, organic acid treatment and dealumination and silicon replenishment, modified ZSM-5 molecular sieve with suitable molar ratio of SiO2/Al2O3 is prepared to reduce the outer surface and mesoporous acid and increase the mesoporous pore volume. Fixed-point removal of the acid center of the zigzag pore improves the selectivity and stability of the catalyst.
The liquid collection and liquid wax yield of the device is improved, multiple cracking is reduced, the paraposition selectivity and reaction stability of the catalyst are improved, the waste of silicone is reduced, and the process is simplified.
Smart Images

Figure CN116062767B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of molecular sieves and preparation thereof, and in particular to a modified ZSM-5 molecular sieve and a preparation method and application thereof. Background Art
[0002] Benzene is alkylated with linear olefins (C10-14) to produce linear alkylbenzene, which is an intermediate for producing linear alkylbenzene sulfonic acid, which is an important monomer of biodegradable detergent. In the 1940s, people found that linear alkylbenzene sulfonic acid has better surface activity than soap, is cheap, and has good decontamination ability in a wide molecular weight range (C10-14). As a result, alkylbenzene detergents have developed rapidly. However, early alkylbenzenes have branches on their long chains. As we all know, detergents produced with branched alkylbenzenes will form foam in rivers, lakes and seas for a long time after use, which is difficult to eliminate, thus causing serious environmental pollution. The reason is that branched alkylbenzenes are not easily biodegradable, so their surface activity exists for a long time; while linear alkylbenzenes are easily biodegradable. If they are used as detergents, environmental pollution can be greatly reduced. In addition, linear alkylbenzenes also have the characteristics of good processing performance, good color of sulfonates, good solubility, high purity, low non-alkylbenzene content and high linearity.
[0003] In recent years, with the rapid development of coal chemical industry, the development of indirect liquefaction and direct liquefaction technology of coal-to-oil in China, the α-olefin or linear alkane rich in indirect liquefaction of coal-to-oil has also been widely used as the raw material for synthesizing alkylbenzene. Wang Zeyun et al. used alkylbenzene prepared from alkylbenzene olefins after cutting as raw material, and then obtained coal-to-alkylbenzene sulfonate after sulfonation and neutralization, which has better performance than traditional petroleum benzene sulfonate, and various indicators meet the requirements of national standards. CN106281444A designed a method of using light distillate oil and heavy distillate oil produced by the Fischer-Tropsch synthesis unit of Inner Mongolia Yitai Coal-to-Oil Company as raw materials, and fractionated stable light hydrocarbons and liquid paraffin products after hydrogenation pre-refining and hydrorefining, and its normal alkanes are greater than 92%. The carbon chain length distribution range of Fischer-Tropsch synthetic oil is very wide, about C1-C80. The amount of straight-chain alkylbenzene raw material, namely liquid paraffin, obtained by distillation is limited. Selective cracking of Fischer-Tropsch synthetic wax with a higher carbon number to obtain liquid paraffin is an effective way to increase the production of liquid paraffin, but no relevant research has been reported so far.
[0004] The ZSM-5 molecular sieve has a three-dimensional double ten-membered ring pore structure, which is a straight and sinusoidal pore. The two sets of ten-membered ring pores are orthogonal. The straight ten-membered ring pores are parallel to the b axis, with a pore size of 0.53×0.56nm, and the sinusoidal ten-membered ring pores are parallel to the a axis, with a pore size of 0.51×0.55nm. This pore structure feature gives it shape-selective catalytic performance. The molecular dynamics size of most isomeric paraffins is larger than the pores of the ZSM-5 molecular sieve and cannot be formed in the ZSM-5 molecular sieve, so that the ZSM-5 molecular sieve can be used in the hydrocracking of Fischer-Tropsch wax with a very high content of normal hydrocarbons to produce linear alkylbenzene raw materials, that is, liquid paraffin products. However, the presence of acidity on the pores and outer surfaces in the ZSM-5 molecular sieve raw powder will cause side reactions, affecting its catalytic performance.
[0005] In order to obtain a catalyst with high para-selectivity and reaction stability, the ZSM-5 molecular sieve must be modified. Among them, silanization of molecular sieves is a frequently used and relatively effective method for modifying the acidity of the outer surface. According to public information reports, the current silanization can be divided into the following methods: (1) vacuum chemical vapor deposition method; (2) flow chemical vapor deposition method; (3) liquid phase chemical impregnation method; (4) reflux liquid phase deposition method; (5) chemical reaction deposition method. Although the process is different, the main purpose is to load amorphous silica on the outer surface of the molecular sieve by deposition to eliminate the acidic center on the outer surface. However, traditional silanization methods require repeated and cyclic impregnation to achieve the purpose of eliminating the acidity of the outer surface, resulting in a large amount of waste of silicone esters and greatly reducing the efficiency of the modification process. Although the improved chemical reaction deposition method improves the modification efficiency and silicone ester utilization rate, it requires special operations, making the process cumbersome and inevitably causing pore blockage. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a modified ZSM-5 molecular sieve and its preparation method and application. The catalyst prepared by the modified ZSM-5 molecular sieve is used for the hydrocracking of Fischer-Tropsch wax to produce linear alkylbenzene raw materials, which can greatly improve the liquid recovery and liquid wax recovery of the device.
[0007] The first aspect of the present invention provides a modified ZSM-5 molecular sieve, wherein the outer surface SiO2 / Al2O3 molar ratio of the modified ZSM-5 molecular sieve is 260-2000, the bulk SiO2 / Al2O3 molar ratio is 20-100, the total infrared acid content of pyridine is 0.20-0.60 mmol / g, and the total infrared acid content of di-tert-butylpyridine is 0.001-0.05 mmol / g.
[0008] Furthermore, the mesopore volume of the modified ZSM-5 molecular sieve accounts for 20% to 50% of the total pore volume, preferably 21% to 48%.
[0009] Furthermore, preferably, the outer surface SiO2 / Al2O3 molar ratio of the modified ZSM-5 molecular sieve is 400-1000, and the bulk SiO2 / Al2O3 molar ratio is 20-48.
[0010] Further, preferably, the total IR acid content of pyridine in the modified ZSM-5 molecular sieve is 0.30-0.50 mmol / g, and the total IR acid content of di-tert-butylpyridine is 0.02-0.03 mmol / g.
[0011] Furthermore, the mesopore volume of the modified ZSM-5 molecular sieve accounts for 20% to 50% of the total pore volume, including but not limited to 20%, 21%, 23%, 25%, 30%, 35%, 36%, 40%, 42%, 44%, 45%, 48%, etc.
[0012] Furthermore, the mesopores in the modified ZSM-5 molecular sieve are concentrated in the range of 2 to 20 nm, wherein the volume of mesopores in the range of 2 to 20 nm accounts for 70% to 95% of the total volume of mesopores. In the present invention, mesopores refer to pores with a pore size of 2 to 50 nm.
[0013] The second aspect of the present invention provides a method for preparing a modified ZSM-5 molecular sieve, comprising the following steps:
[0014] (1) Performing pore expansion treatment on ZSM-5 molecular sieve;
[0015] (2) impregnating the material molecular sieve obtained in step (1) with a pore protection liquid;
[0016] (3) treating the material obtained in step (2) with an organic acid;
[0017] (4) mixing the material obtained in step (3) with a dealumination and siliconization agent to carry out dealumination and siliconization;
[0018] (5) The material obtained in step (4) is filtered, washed, dried and calcined to obtain a modified ZSM-5 molecular sieve.
[0019] Furthermore, in step (1), the ZSM-5 molecular sieve can be a commercially available product or a microporous hydrogen-type ZSM-5 molecular sieve prepared according to the prior art. The properties of the ZSM-5 molecular sieve are as follows: SiO2 / Al2O3 molar ratio of 30 to 100, specific surface area of 300 to 450 m 2 / g, pore volume is 0.15~0.20cm 3 / g.
[0020] In the method of the present invention, in step (1), the pore expansion treatment can be a pore expansion method such as alkali treatment. The alkaline solution used in the alkali treatment is one or more of NaOH solution, KOH solution, and quaternary ammonium salt solution. The concentration of the alkaline solution is 0.1-1.0 mol / L. The liquid-to-solid volume ratio of the alkaline solution to the ZSM-5 molecular sieve is (6-10): 1 mL / g. The temperature of the alkali treatment is 40°C-70°C, and the time of the alkali treatment is 0.5h-2h.
[0021] In the method of the present invention, in step (1), the pore expansion treatment process is as follows: placing the ZSM-5 molecular sieve in an alkaline solution, stirring, filtering, and repeating this process 2 to 4 times; then washing with deionized water and drying.
[0022] Furthermore, in step (1), the washing is performed 1 to 5 times until the alkali metal ion content is less than 0.1 wt%.
[0023] Furthermore, in step (2), the pore protection solution is one or more of isopropylamine solution, tetraethylammonium hydroxide solution, tetrapropylammonium hydroxide solution, etc. The concentration of the pore protection agent solution is 0.2-2.0 mol / L, preferably 0.4-1.5 mol / L.
[0024] Furthermore, in step (2), the impregnation is preferably equal volume impregnation. The impregnation temperature is room temperature, generally 20-25°C.
[0025] Furthermore, in step (3), the organic acid is one or more of 2,4-dimethylbenzenesulfonic acid and 2,5-dimethylbenzoic acid.
[0026] Furthermore, in step (3), the specific operation is as follows: first, the material obtained in step (2) is mixed with water, wherein the liquid-solid ratio of water to the material obtained in step (2) is 2:1 to 6:1 mL / g, and then an organic acid is added until the pH value of the solution drops below 8, preferably 6.5 to 7.5.
[0027] Furthermore, in step (4), the dealuminizing and siliconizing agent is at least one of ammonium hexafluorosilicate solution, ethyl orthosilicate solution, etc. The molar concentration of the dealuminizing and siliconizing agent is 0.3 to 1.0 mol / L. The mass ratio of the material obtained in step (3) to the dealuminizing and siliconizing agent is 1:1 to 1:5.
[0028] Furthermore, the specific operation process of step (4) is: quickly heating the material obtained in step (3) to 60-100°C, and continuously stirring, adding the dealumination and siliconization reagent dropwise, and continuing to stir for 60-120 minutes after the addition is completed. The addition speed is not more than 0.5 mL / min·g of the material obtained in step (3); preferably 0.2-0.4 mL / min·g of the material obtained in step (3).
[0029] Furthermore, in step (5), the filtering and washing can be carried out by conventional methods in the art, the drying temperature is 100°C to 150°C, and the drying time is 2 to 4 hours; the roasting temperature is 400°C to 600°C; and the roasting time is 3 to 5 hours.
[0030] The third aspect of the present invention provides an application of the modified ZSM-5 molecular sieve in the production of liquid paraffin catalyst by hydrocracking of Fischer-Tropsch wax.
[0031] Furthermore, the Fischer-Tropsch wax hydrocracking catalyst comprises the above-mentioned modified ZSM-5 molecular sieve and a Group VIII metal component, wherein, based on the weight of the catalyst, the content of the modified ZSM-5 molecular sieve is 30% to 90%, preferably 40% to 70%, and the content of the Group VIII metal component in terms of oxide is 5% to 40%, preferably 10% to 30%.
[0032] Furthermore, the Group VIII metal is cobalt and / or nickel.
[0033] The application specifically includes: in the presence of hydrogen, the Fischer-Tropsch wax raw material is subjected to a hydrocracking reaction after being hydrorefined, and the reaction conditions are as follows: the reaction pressure is 5.0-8.0 MPa, the hydrogen-oil volume ratio is 400:1-600:1, and the liquid hourly volume space velocity is 0.5-2h -1 , the reaction temperature is 280~400℃.
[0034] Compared with the prior art, the present invention has the following advantages:
[0035] 1. The modified ZSM-5 molecular sieve of the present invention has low amount of di-tert-butylpyridine infrared acid, and eliminates mesoporous acid and external surface acid.
[0036] 2. The modified ZSM-5 molecular sieve of the present invention has a high mesopore content, which is beneficial to the diffusion of long-chain alkanes and reduces multiple cracking.
[0037] 3. The preparation method of the modified ZSM-5 molecular sieve of the present invention removes the acid center in the non-zigzag pores at a fixed point, and most of the aluminum sites in the non-zigzag pores are replaced by non-acidic silicon atoms under the action of ammonium hexafluorosilicate, and the molecular sieve structure is completely retained. The mesopore content is increased by pore expansion treatment, which is conducive to the diffusion of long-chain alkanes and intermediate products and reduces excessive cracking. Isomeric chain hydrocarbons are difficult to form in the microporous pores of the ZSM-5 molecular sieve, and the product is mainly normal alkanes, which greatly improves the liquid yield of the device and the yield of liquid paraffin. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1It is the XRD diagram of commercially available ZSM-5 molecular sieve and the modified ZSM-5 molecular sieve Z-T4 obtained in Example 4 of the present invention. DETAILED DESCRIPTION
[0039] The functions and effects of the technical solution of the present invention are further illustrated below in conjunction with embodiments and comparative examples, but the following embodiments do not constitute a limitation on the protection scope of the present invention.
[0040] In the present invention, % involved in the embodiments and comparative examples are all mass fractions unless otherwise specified.
[0041] In the present invention, the outer surface SiO2 / Al2O3 molar ratio is measured by X-ray photoelectron spectroscopy (XPS), and the element composition and state of the catalyst surface are measured on a Multilab2000 electron spectrometer of Thermofisher Company of the United States, the excitation source is Mg Kα, and the cathode voltage and current are 13kV and 20mA respectively. The electron binding energy is calibrated by C1s (284.6eV).
[0042] In the present invention, the bulk SiO2 / Al2O3 molar ratio is obtained by X-ray fluorescence spectroscopy (XRF) analysis using a ZSX100e X-ray fluorescence spectrometer, with a Kα spectral line, Li F1 crystal, Rh target, SC scintillation detector, 20s timing, and a vacuum optical path atmosphere.
[0043] In the present invention, the specific surface area, pore volume and pore distribution are measured by the following method: using ASAP 2420 low-temperature liquid nitrogen physical adsorption instrument produced by MICROMERITICS Corporation of the United States, with a pretreatment temperature of 300° C. and a pretreatment time of 4 hours.
[0044] In the present invention, the pyridine infrared determination method is as follows: the powdered ZSM-5 molecular sieve is pressed into tablets, vacuumed, and then degassed at 450° C. for 2 hours. When the temperature drops to room temperature, the pyridine molecule is used as a probe molecule to measure the infrared spectrum of chemical desorption and calculate the adsorption amount.
[0045] In the present invention, the total infrared acid amount of di-tert-butylpyridine refers to the kinetic diameter of The 2,6-di-tert-butylpyridine molecule can contact the proton acid. The infrared determination method of 2,6-di-tert-butylpyridine is as follows: the powdered ZSM-5 molecular sieve is pressed into a tablet, evacuated, and degassed at 450°C for 2 hours. When the temperature drops to room temperature, the 2,6-di-tert-butylpyridine molecule is used as a probe molecule to measure its infrared spectrum of chemical desorption and calculate the adsorption amount.
[0046] The ZSM-5 raw powder involved in the embodiments and comparative examples of the present invention is a commercially available product purchased, which is a microporous hydrogen-type ZSM-5 molecular sieve. The properties of the ZSM-5 are as follows: the specific surface area is 405m2 / g, pore volume is 0.182cm 3 / g, water absorption is 55%, and SiO2 / Al2O3 ratio (molar) is 31.2.
[0047] Example 1
[0048] 180mL of 0.1mol / L NaOH solution was added to 30g of commercially available ZSM-5 raw powder, stirred, heated to 60℃, stirred continuously for 60min, filtered and dried. 16.5mL of 0.2mol / L isopropylamine solution was used to impregnate the obtained material in equal volume, and allowed to stand for 10min; 170mL of water was added, 2,5-xylenesulfonic acid was added dropwise until the pH value was 7.0, stirred and heated to 60℃, and 90mL of 0.3mol / L ammonium hexafluorosilicate solution was added dropwise with a peristaltic pump at a uniform speed, with a drop rate of 0.2mL / min·g, and the temperature was maintained at 60℃ and stirred continuously for 90min. Filter while hot, add 300mL of water to the obtained filter cake, heat to 60℃ and maintain for 20min, filter while hot, dry the filter cake at 120℃ for 24h, and calcine at 500℃ for 3h to obtain the modified molecular sieve, named Z-T1.
[0049] Example 2
[0050] 180mL of 0.3mol / L NaOH solution was added to 30g of commercially available ZSM-5 raw powder, stirred, heated to 60℃, stirred continuously for 60min, filtered and dried. 16.5mL of 0.6mol / L isopropylamine solution was used to impregnate the obtained material in equal volume, and allowed to stand for 10min; 170mL of water was added, 2,5-xylenesulfonic acid was added dropwise until the pH value was 7.0, stirred and heated to 60℃, 90mL of 0.3mol / L ammonium hexafluorosilicate solution was added dropwise at a constant speed using a peristaltic pump, the drop rate was 0.2mL / min·g, the temperature was maintained at 60℃ and stirred continuously for 90min. Filter while hot, add 300mL of water to the obtained filter cake, heat to 60℃ and maintain for 20min, filter while hot, dry the filter cake at 120℃ for 24h, and calcine at 500℃ for 3h to obtain the modified molecular sieve, named Z-T2.
[0051] Example 3
[0052] 180mL of 0.4mol / L NaOH solution was added to 30g of commercially available ZSM-5 raw powder, stirred, heated to 60℃, stirred continuously for 60min, filtered and dried. 16.5mL of 0.6mol / L isopropylamine solution was used to impregnate 30g of the obtained material in equal volume, and allowed to stand for 10min; 170mL of water was added, 2,5-xylenesulfonic acid was added dropwise until the pH value was 6.5, stirred and heated to 60℃, and 90mL of 0.3mol / L ammonium hexafluorosilicate solution was added dropwise at a constant speed with a peristaltic pump, the drop rate was 0.2mL / min·g, the temperature was maintained at 60℃ and stirred continuously for 90min. Filter while hot, add 300mL of water to the obtained filter cake, heat to 60℃ and maintain for 20min, filter while hot, dry the filter cake at 120℃ for 24h, and calcine at 500℃ for 3h to obtain the modified molecular sieve, named Z-T3.
[0053] Example 4
[0054] 180mL of 0.5mol / L NaOH solution was added to 30g of commercially available ZSM-5 raw powder, stirred, heated to 60℃, stirred continuously for 60min, filtered and dried. 16.5mL of 0.8mol / L isopropylamine solution was used to impregnate the obtained material in equal volume, and allowed to stand for 10min; 170mL of water was added, 2,5-xylenesulfonic acid was added dropwise until the pH value was 6.0, stirred and heated to 60℃, 90mL of 0.3mol / L ammonium hexafluorosilicate solution was added dropwise at a constant speed using a peristaltic pump, the drop rate was 0.2mL / min·g, the temperature was maintained at 60℃ and stirred continuously for 90min. Filter while hot, add 300mL of water to the obtained filter cake, heat to 60℃ and maintain for 20min, filter while hot, dry the filter cake at 120℃ for 24h, and calcine at 500℃ for 3h to obtain the modified molecular sieve, named Z-T4.
[0055] Example 5
[0056] 180mL of 0.6mol / L NaOH solution was added to 30g of commercially available ZSM-5 raw powder, stirred, heated to 60℃, stirred continuously for 60min, filtered and dried. 16.5mL of 1.0mol / L isopropylamine solution was used to impregnate the obtained material in equal volume, and it was allowed to stand for 10min; 170mL of water was added, 2,5-xylenesulfonic acid was added dropwise until the pH value was 7.0, stirred and heated to 60℃, 90mL of 0.3mol / L ammonium hexafluorosilicate solution was added dropwise at a constant speed with a peristaltic pump, the drop rate was 0.2mL / min·g, the temperature was maintained at 60℃ and stirred continuously for 90min. Filter while hot, add 300mL of water to the obtained filter cake, heat to 60℃ and keep it for 20min, filter while hot, dry the filter cake at 120℃ for 24h, and calcine at 500℃ for 3h to obtain the modified molecular sieve, named Z-T5.
[0057] Example 6
[0058] 180mL of 0.6mol / L NaOH solution was added to 30g of commercially available ZSM-5 raw powder, stirred, heated to 60℃, stirred continuously for 60min, filtered and dried. 16.5mL of 1.2mol / L isopropylamine solution was used to impregnate 30g of the obtained material in equal volume, and the mixture was allowed to stand for 10min; 170mL of water was added, 2,5-xylenesulfonic acid was added dropwise until the pH value was 7.0, stirred and heated to 60℃, 90mL of 0.3mol / L ammonium hexafluorosilicate solution was added dropwise at a constant speed using a peristaltic pump, the drop rate was 0.2mL / min·g, the temperature was maintained at 60℃ and stirred continuously for 90min. Filtered while hot, 300mL of water was added to the obtained filter cake, heated to 60℃ and maintained for 20min, filtered while hot, the filter cake was dried at 120℃ for 24h, and then calcined at 500℃ for 3h. The obtained modified molecular sieve was named Z-T6.
[0059] Example 7
[0060] 180mL of 0.7mol / L NaOH solution was added to 30g of commercially available ZSM-5 raw powder, stirred, heated to 60℃, stirred continuously for 60min, filtered and dried. 16.5mL of 1.4mol / L isopropylamine solution was used to impregnate the obtained material in equal volume, and it was allowed to stand for 10min; 170mL of water was added, 2,5-xylenesulfonic acid was added dropwise until the pH value was 6.5, stirred and heated to 60℃, and 90mL of 0.3mol / L ammonium hexafluorosilicate solution was added dropwise at a constant speed with a peristaltic pump, the drop rate was 0.2mL / min·g, the temperature was maintained at 60℃ and stirred continuously for 90min. Filter while hot, add 300mL of water to the obtained filter cake, heat to 60℃ and keep it for 20min, filter while hot, dry the filter cake at 120℃ for 24h, and calcine at 500℃ for 3h to obtain the modified molecular sieve, named Z-T7.
[0061] Example 8
[0062] 180mL of 0.9mol / L NaOH solution was added to 30g of commercially available ZSM-5 raw powder, stirred, heated to 60℃, stirred continuously for 60min, filtered and dried. 16.5mL of 1.8mol / L isopropylamine solution was used to impregnate the obtained material in equal volume, and it was allowed to stand for 10min; 170mL of water was added, 2,5-xylenesulfonic acid was added dropwise until the pH value was 6.0, stirred and heated to 60℃, and 90mL of 0.3mol / L ammonium hexafluorosilicate solution was added dropwise with a peristaltic pump at a uniform speed, the drop rate was 0.2mL / min·g, the temperature was maintained at 60℃ and stirred continuously for 90min. Filter while hot, add 300mL of water to the obtained filter cake, heat to 60℃ and keep it for 20min, filter while hot, dry the filter cake at 120℃ for 24h, and calcine at 500℃ for 3h to obtain the modified molecular sieve, named Z-T8.
[0063] Comparative Example 1
[0064] 30g of commercial molecular sieve ZSM-5 powder was added with 170mL of water, stirred and heated to 65°C, and 90g of 0.6mol / L ammonium hexafluorosilicate solution was added dropwise at a constant speed using a peristaltic pump for 10min, and the temperature was maintained at 65°C and stirred for 90min. Filtered while hot, 300mL of water was added to the filter cake, heated to 60°C and maintained for 20min, filtered while hot, dried the filter cake at 120°C for 24h, and calcined at 500°C for 3h. The modified molecular sieve was named ZB.
[0065] Comparative Example 2
[0066] Prepare an isopropylamine solution with a concentration of 1.2 mol / L, take 16.5 mL of the solution and use it to soak 30 g of ZSM-5 raw powder in equal volume, and mix well. Add 170 mL of water, stir and heat to 65 ° C, use a peristaltic pump to uniformly add 90 g of 0.6 mol / L ammonium hexafluorosilicate solution, the addition time is 10 min, the temperature is maintained at 65 ° C and stirring is continued for 90 min. Filter while hot, add 300 mL of water to the filter cake, heat to 60 ° C and maintain for 20 min, filter while hot, dry the filter cake at 120 ° C for 24 h, and calcine at 500 ° C for 3 h. The modified molecular sieve obtained is named ZC.
[0067] Table 1 Characterization results of molecular sieves of examples and comparative examples
[0068]
[0069] Example 9
[0070] The catalyst was prepared by Z-T4, and the preparation process was as follows: Z-T4 and macroporous alumina (specific surface area of 302m 2 / g, pore volume is 0.96cm 3 / g), aluminum sol binder, kneading, extruding and molding, and then drying and calcining to obtain a carrier; the above-mentioned carrier is impregnated with an impregnation solution containing nickel nitrate, and then dried and calcined to obtain a catalyst, recorded as C1; wherein the mass fraction of Z-T4 is 50wt%, the mass fraction of macroporous alumina is 20wt%, the mass fraction of NiO is 25wt%, and the rest is a binder.
[0071] 10 g of catalyst C1 was placed in a fixed bed reactor at a reaction pressure of 6.0 MPa, a hydrogen-to-oil volume ratio of 500:1, and a liquid hourly volume space velocity of 10 h -1 At a reaction temperature of 320°C, Fischer-Tropsch wax refined reduced base oil was used as raw material. The raw material properties are shown in Table 2, and the evaluation results are shown in Table 3.
[0072] Example 10
[0073] The catalyst was prepared by Z-T5, and the preparation process was as follows: Z-T5 and macroporous alumina (specific surface area of 302m 2 / g, pore volume is 0.96cm 3 / g), aluminum sol binder, kneading, extruding and molding, and then drying and calcining to obtain a carrier; the above-mentioned carrier is impregnated with an impregnation solution containing nickel nitrate, and then dried and calcined to obtain a catalyst, recorded as C2; wherein the mass fraction of Z-T5 is 50wt%, the mass fraction of macroporous alumina is 20wt%, the mass fraction of NiO is 25wt%, and the rest is a binder.
[0074] 10 g of catalyst C2 was placed in a fixed bed reactor at a reaction pressure of 6.0 MPa, a hydrogen-to-oil volume ratio of 500:1, and a liquid hourly volume space velocity of 10 h -1 At a reaction temperature of 320°C, Fischer-Tropsch wax refined reduced base oil was used as raw material. The raw material properties are shown in Table 2, and the evaluation results are shown in Table 3.
[0075] Comparative Example 3
[0076] The catalyst was prepared by ZB, and the preparation process was as follows: ZB and macroporous alumina (specific surface area of 302m 2 / g, pore volume is 0.96cm 3 / g) and aluminum sol binder are kneaded, extruded and formed, and then dried and calcined to obtain a carrier; the above-mentioned carrier is impregnated with an impregnation solution containing nickel nitrate, and then dried and calcined to obtain a catalyst, which is recorded as CB1; wherein the mass fraction of ZB is 50wt%, the mass fraction of macroporous alumina is 20wt%, the mass fraction of NiO is 25wt%, and the rest is a binder.
[0077] 10 g of catalyst CB1 was placed in a fixed bed reactor at a reaction pressure of 6.0 MPa, a hydrogen-to-oil volume ratio of 500:1, and a liquid hourly volume space velocity of 10 h -1 At a reaction temperature of 320°C, FT synthetic oil hydrotreating minus two-line was used as raw material. The raw material properties are shown in Table 2, and the evaluation results are shown in Table 3.
[0078] Comparative Example 4
[0079] The catalyst was prepared by ZC, and the preparation process was as follows: ZC and macroporous alumina (specific surface area of 302m 2 / g, pore volume is 0.96cm 3 / g), aluminum sol binder, kneading, extruding and molding, and then drying and calcining to obtain a carrier; the above-mentioned carrier is impregnated with an impregnation solution containing nickel nitrate, and then dried and calcined to obtain a catalyst, recorded as CB2; wherein the mass fraction of ZC is 50wt%, the mass fraction of macroporous alumina is 20wt%, the mass fraction of NiO is 25wt%, and the rest is a binder.
[0080] 10 g of catalyst CB2 was placed in a fixed bed reactor at a reaction pressure of 6.0 MPa, a hydrogen-to-oil volume ratio of 500:1, and a liquid hourly volume space velocity of 10 h -1 At a reaction temperature of 320°C, FT synthetic oil hydrotreating minus two-line was used as raw material. The raw material properties are shown in Table 2, and the evaluation results are shown in Table 3.
[0081] Table 2 Raw oil properties
[0082] Raw oil name Fischer-Tropsch synthesis line <![CDATA[Density (20 °C) / g·cm -3 > 0.782 Distillation range / ℃ IBP / 10% 310 / 326 50% / 90% 343 / 364 95% / EBP 371 / 375
[0083] Table 3 Comparative evaluation results of catalyst performance of examples and comparative examples
[0084] Catalyst No. C1 C2 CB1 CB2 Liquid yield of the device, wt% 99.2 97.3 92.5 90.6 Liquid wax yield, wt% 65.1 58.3 51.2 48.6
Claims
1. A modified ZSM-5 molecular sieve, characterized in that: The modified ZSM-5 molecular sieve has an outer surface SiO2 / Al2O3 molar ratio of 260-2000, a bulk SiO2 / Al2O3 molar ratio of 20-100, a pyridine infrared total acid content of 0.20-0.60 mmol / g, and a di-tert-butylpyridine infrared total acid content of 0.001-0.05 mmol / g.
2. The modified ZSM-5 molecular sieve according to claim 1, characterized in that: The mesopore volume of the modified ZSM-5 molecular sieve accounts for 20% to 50% of the total pore volume.
3. The modified ZSM-5 molecular sieve according to claim 2, characterized in that: The mesopore volume of the modified ZSM-5 molecular sieve accounts for 21% to 48% of the total pore volume.
4. The modified ZSM-5 molecular sieve according to claim 1, characterized in that: The outer surface SiO2 / Al2O3 molar ratio of the modified ZSM-5 molecular sieve is 400-1000, and the bulk SiO2 / Al2O3 molar ratio is 20-48; and / or, the total infrared acid content of pyridine of the modified ZSM-5 molecular sieve is 0.30-0.50 mmol / g, and the total infrared acid content of di-tert-butylpyridine is 0.02-0.03 mmol / g.
5. The modified ZSM-5 molecular sieve according to claim 1, characterized in that: The pore volume of mesopores with a size of 2 to 20 nm in the modified ZSM-5 molecular sieve accounts for 70% to 95% of the total pore volume of mesopores.
6. A method for preparing the modified ZSM-5 molecular sieve according to any one of claims 1 to 5, comprising the following steps: (1) Performing pore expansion treatment on ZSM-5 molecular sieve; (2) impregnating the material molecular sieve obtained in step (1) with a pore protection liquid; (3) treating the material obtained in step (2) with an organic acid; (4) mixing the material obtained in step (3) with a dealumination and siliconization agent to carry out dealumination and siliconization; (5) The material obtained in step (4) is filtered, washed, dried and calcined to obtain a modified ZSM-5 molecular sieve.
7. The method according to claim 6, characterized in that: In step (1), the pore expansion treatment is an alkali treatment; the alkaline solution used is one or more of a NaOH solution, a KOH solution, and a quaternary ammonium salt solution; the liquid-to-solid volume ratio of the alkaline solution to the ZSM-5 molecular sieve is (6-10): 1 mL / g; the temperature of the alkali treatment is 40° C. to 70° C., and the time of the alkali treatment is 0.5 h to 2 h.
8. The method according to claim 7, characterized in that: In step (1), the pore expansion process is as follows: placing the ZSM-5 molecular sieve in an alkaline solution, stirring, filtering, and repeating this process 2 to 4 times; then washing with deionized water and drying.
9. The method according to claim 6, characterized in that: In step (2), the pore protection solution is one or more of isopropylamine solution, tetraethylammonium hydroxide solution, and tetrapropylammonium hydroxide solution; the concentration of the pore protection solution is 0.2 to 2.0 mol / L.
10. The method according to claim 6, characterized in that: In step (3), the organic acid is one or more of 2,4-dimethylbenzenesulfonic acid and 2,5-dimethylbenzoic acid.
11. The method according to claim 6, characterized in that: The specific operation of step (3) is as follows: first, the material obtained in step (2) is mixed with water, wherein the liquid-solid ratio of water to the material obtained in step (2) is 2:1 to 6:1 mL / g, and then an organic acid is added until the pH value of the solution drops below 8.
12. The method according to claim 11, characterized in that: Add organic acid until the pH of the solution drops to 6.5-7.
5.
13. The method according to claim 6, characterized in that: In step (4), the dealuminizing and siliconizing reagent is at least one of an ammonium hexafluorosilicate solution and an ethyl orthosilicate solution; the molar concentration of the dealuminizing and siliconizing reagent is 0.3 to 1.0 mol / L; wherein the mass ratio of the material obtained in step (3) to the dealuminizing and siliconizing reagent is 1:1 to 1:
5.
14. The method according to claim 6, characterized in that: The specific operation process of step (4) is: quickly heating the material obtained in step (3) to 60-100° C., and continuously stirring, and adding a dealuminizing and siliconizing reagent dropwise, and continuing to stir for 60-120 minutes after the addition is completed.
15. Use of the modified ZSM-5 molecular sieve according to any one of claims 1 to 5 or the modified ZSM-5 molecular sieve prepared by the method according to any one of claims 6 to 14 in the catalyst for producing liquid paraffin by hydrocracking of Fischer-Tropsch wax.
16. The use according to claim 15, characterized in that: The Fischer-Tropsch wax raw material is subjected to hydrocracking reaction after being hydrorefined. The reaction conditions are as follows: reaction pressure is 5.0-8.0 MPa, hydrogen-oil volume ratio is 400:1-600:1, liquid hourly volume space velocity is 0.5-2 h -1 , the reaction temperature is 280~400℃.