A kind of resistive wave absorbing film and its preparation method and application
By using a mixed carbon slurry composed of benzoxazine resin, epoxy resin and anhydride curing agent, a high-temperature resistance type wave absorbing film was prepared, which solved the problems of the thickness and weight of the existing wave absorbing material and achieved high performance The wave absorption effect and stable resistance value are suitable for the preparation of composite functional materials.
Patent Information
- Application Number
- CN202211723982.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The existing absorbent materials have shortcomings in thickness, weight, high temperature resistance and tensile strength, which leads to limited application. The application and silk screening methods are prone to insufficient high temperature resistance, low tensile strength and peel strength, and corrosion resistance. The problem of insufficient performance leads to unstable wave absorption effect.
Using a mixed carbon slurry composed of benzoxazine resin, epoxy resin, anhydride curing agent and conductive powder, a resistive wave absorbing film is prepared through silk screen printing technology, and the heat resistance of benzoxazine resin and the adhesion of epoxy resin are used. The junction strength forms an interpenetrating network structure, improves mechanical and impact resistance, and improves thermal and humid and heat aging performance through the use of anhydride curing agent.
The prepared resistive wave absorbing film has high high temperature resistance, good impact resistance, adhesive performance and stable resistance. The flat tensile strength exceeds 1.5MPa, high temperature resistance exceeds 180℃, and the resistance value can be adjusted. It is suitable for Preparation of composite functional absorbing materials.
Smart Images

Figure CN116063723B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of absorbing materials, and in particular to a resistive absorbing film and a preparation method and application thereof. Background Art
[0002] With the rapid development of target detection technology, the requirements for absorbing materials are getting higher and higher, requiring materials to be light in weight, thin in thickness, with wide absorption frequency band and strong absorption peak. According to the electromagnetic loss mechanism, absorbing materials can be mainly divided into resistive type, dielectric type and magnetic dielectric type. At present, the commonly used method for preparing absorbing materials is to disperse the absorbent in the material to make a corrugated or pyramidal structure, but in many fields, the application is limited due to the thickness or weight of the absorbing material. There are also methods of smearing and screen printing, where the mixed carbon paste is screen-printed on the carrier to prepare the absorbing material, but it is easy to have many problems such as insufficient high temperature resistance, low tensile strength and peel strength, insufficient corrosion resistance, and great changes in resistance after bonding and compounding other materials, resulting in unstable absorbing effect and failure to meet performance requirements. Its application is also subject to certain restrictions. Therefore, there is an urgent need for an absorbing material with high temperature resistance, controllable resistance and excellent performance. Summary of the invention
[0003] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a high temperature resistant, controllable resistance, excellent performance resistive absorbing film and a preparation method and application thereof.
[0004] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0005] A resistive wave-absorbing film is mainly prepared from a mixed carbon slurry and a film carrier. The mixed carbon slurry comprises the following components by weight: 10 to 15 parts of benzoxazine resin, 25 to 40 parts of epoxy resin, 0.1 to 5 parts of an auxiliary agent, 10 to 15 parts of a solvent, 15 to 35 parts of an acid anhydride curing agent and 10 to 35 parts of a conductive powder.
[0006] Preferably, the epoxy resin is bisphenol A epoxy resin; the solvent includes one or more of ethylene glycol butyl ether acetate, dimethyl glutarate, and dimethyl succinate; the anhydride curing agent includes one or more of liquid methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, and methylnadic anhydride. The solvent is a high boiling point solvent, which evaporates slowly at room temperature, and can ensure that the viscosity of the slurry is more stable during the printing process.
[0007] The epoxy resin and a sufficient amount of anhydride are cured under the action of an auxiliary agent. After the epoxy resin is completely cured, benzoxazine undergoes ring-opening polymerization under high temperature to form an interpenetrating network structure, thereby effectively improving the mechanical and impact resistance, thermal properties, and wet-heat aging properties of the epoxy resin cross-linked anhydride curing agent.
[0008] Because benzoxazine resin (BEP) has the characteristics of heat resistance, flame retardancy, low shrinkage and good mechanical properties, epoxy resin has the characteristics of high bonding strength and cohesive strength, excellent corrosion resistance and dielectric properties, and anhydride curing agent has the characteristics of small curing shrinkage, high curing heat deformation temperature, excellent mechanical and electrical properties, and this curing agent cures very slowly at room temperature and can be stored for a long time, the three work together to improve the heat resistance, corrosion resistance and other properties of the absorbing film.
[0009] Preferably, the auxiliary agent includes a combination of one or more of a dispersant, a defoamer, and a promoter; the dispersant is a BYK polymer wetting dispersant, and the weight portion of the dispersant is 1 to 4 parts; the defoamer is tributyl phosphate, and the weight portion of the defoamer is 0.1 to 0.5 parts; the promoter is an imidazole promoter, and the imidazole promoter includes a combination of one or more of 2-methylimidazole, 2-ethyl-4-methylimidazole, and 2-phenylimidazole, and the weight portion of the promoter is 0.1 to 0.5 parts.
[0010] Preferably, the conductive powder is a mixture of carbon black particles and graphite particles, the carbon black particles are highly conductive carbon black particles with a radius of 0.5 μm to 8 μm; the radius of the graphite particles is 0.5 μm to 5 μm, and the mixing mass ratio of the carbon black particles to the graphite particles is 1:1 to 8. More preferably, the mixing mass ratio of the carbon black particles to the graphite particles is 1:4.
[0011] Preferably, the film carrier is one of FR4 film and PI film, and the thickness of the film carrier is ≤0.1mm and the surface density is ≤100g / m 2 . Choose light, high temperature resistant materials as carriers. The materials are functional materials that can attenuate and effectively eliminate electromagnetic wave energy. When electromagnetic waves are incident in space, induced currents can be generated on the surface. The currents are blocked inside the material and generate internal energy, thereby converting electromagnetic waves into heat energy, which attenuates and eliminates the electromagnetic waves. The carrier materials are all high temperature resistant film materials, which can effectively improve the high temperature resistance of the electronic absorbing film. Moreover, the light and thin carriers can further ensure that the overall thickness of the absorbing film is small, which is more conducive to the stability of the resistance.
[0012] Based on the general inventive concept, the present invention also provides a method for preparing a resistive absorbing film, comprising the following steps: heating and mixing benzoxazine resin and epoxy resin evenly, adding solvent, acid anhydride curing agent and auxiliary agent after cooling and mixing evenly, adding conductive powder to disperse and grind to obtain mixed carbon slurry, screen printing the mixed carbon slurry on a film carrier, and curing to obtain the resistive absorbing film. The carbon slurry is coated on the film to form a conductive layer, wherein the conductive layer itself is resistant to high temperature above 180°C, and the substrate is also resistant to high temperature, and the formed resistive absorbing film has high temperature resistance.
[0013] Preferably, the heating and mixing is to maintain the temperature below 70° C. for stirring; the cooling is to cool to room temperature; the dispersing is performed by a disperser with a speed of 600 to 1200 r / min; and the grinding is performed by a three-roll grinder for 2 to 3 times.
[0014] Preferably, the ambient temperature of the silk screen printing is 18-28°C, and the silk screen printing adopts a silk screen printer. The parameters of the silk screen printer are: the hardness of the scraper is 65-80°, the pressure of the scraper is 40-50N, the silk screen screen is any one of a steel screen screen or a polyester screen screen, and the mesh number is 200-300 meshes; the moving speed of the scraper is 80-200mm / s, and the moving speed of the ink return knife is 240mm / s. The silk screen printer includes a scraper, a silk screen screen, and a scraper. The scraper applies a certain pressure to the conductive paste on the silk screen screen, and at the same time, the scraper moves at a uniform speed toward the other end of the silk screen screen. The conductive paste is squeezed from the mesh to the carrier by the scraper during movement to form an absorbing film. Too low pressure hardness of the scraper affects the printing accuracy, and the service life is too short. The most suitable mesh number is 200-300 mesh. If the mesh number is too small, the mesh size will be large and the slurry will easily pass through the screen. If the mesh number is too large, the powder particles will find it difficult to pass through the screen by the squeegee.
[0015] Preferably, the curing process is: hot stamping at 80-90°C for 3-5 minutes, and then curing at 150-160°C for 0.5-3 hours. Hot stamping at 80-90°C can volatilize most of the solvent, and curing at 150-160°C ensures complete curing.
[0016] Based on the overall inventive concept, the present invention also provides an application of a resistive absorbing film, wherein the resistive absorbing film is attached to polyurethane foam or polymethacrylimide foam to form a composite functional absorbing material or stealth material.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The resistive absorbing film provided by the present invention adopts an ultra-thin high temperature resistant film as a carrier, a high temperature resistant acid anhydride substance as a curing agent, and a benzoxazine resin as a modifier to modify the epoxy resin cross-linked acid anhydride curing agent. The three cooperate with each other. On the one hand, the glass transition temperature and impact strength of the cross-linked product of the epoxy resin and the acid anhydride curing agent can be improved, and the defects of the epoxy resin being brittle and not resistant to impact can be solved, thereby effectively improving the mechanical and impact resistance, thermal properties, wet heat aging properties, and electrical insulation properties of the epoxy resin cross-linked acid anhydride curing agent. On the other hand, the obtained absorbing film has the advantages of high temperature resistance, good impact resistance, good adhesion performance, stable resistance, etc. After testing, the obtained absorbing film has a flat tensile strength of >1.5MPa and a high temperature resistance of >180°C.
[0019] 2. The present invention screen-prints the mixed carbon paste on an ultra-thin carrier for solidification and molding, and uses an ultra-thin high-temperature resistant substrate as a carrier to achieve the properties of light weight, high temperature resistance, corrosion resistance, high bonding strength and the like of the absorbing film, which can be bonded and compounded with a wave-transmitting material to make a structural absorbing material. By controlling the proportion of high-temperature resistant conductive powder, a mixed carbon paste with different resistance values can be prepared, and the mixed carbon paste is screen-printed on an ultra-thin high-temperature resistant carrier to obtain a resistive absorbing film with different resistance values, which can adjust the resistance and improve the high-temperature resistance and tensile strength of the absorbing film. The film has the characteristics of low surface density, high mechanical strength, solvent resistance, high and low temperature resistance, wear resistance, and excellent adhesion. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 This is a physical picture of the resistive absorbing film prepared by the present invention. DETAILED DESCRIPTION
[0022] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0023] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0024] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0025] Embodiment 1:
[0026] A resistive wave absorbing film is prepared by coating a mixed carbon slurry onto a film carrier and curing the mixed carbon slurry. The raw materials of the mixed carbon slurry are configured according to the mass ratio described in Table 1. The highly conductive carbon black particles selected are CaBOT carbon black VXC-72R.
[0027] The method for preparing the resistive wave absorbing film comprises the following steps:
[0028] 1. Add benzoxazine resin and bisphenol A epoxy resin in a flask in proportion, heat to 70°C, stir evenly to obtain a mixed solution in which the resin is completely dissolved, and then cool to room temperature for use;
[0029] 2. Add a fixed proportion of solvent, anhydride curing agent and additives into a stainless steel can according to the table below, adjust the speed to 600-1200r / min, and disperse evenly;
[0030] 3. Add the resin mixture prepared in step 1 to the mixture prepared in step 2 according to the proportion in Table 1 below, then add conductive powder (a mixture of carbon black particles and graphite particles), stir at high speed for 3 hours, transfer to a three-roll grinder and grind 3 times to obtain a mixed carbon slurry for use.
[0031] Table 1: Raw material ratios of Example 1
[0032] Components Mass Highly conductive carbon black particles (2um) 63g Graphite particles (1.7um) 232g Benzoxazine resin BEP 110g Bisphenol A epoxy resin 250g Methyltetrahydrophthalic anhydride MTHPA 185g 2-Ethyl-4-methylimidazole 2E4MZ 2g BYK-163 (BYK brand) 20g Tributyl phosphate 3g Dimethyl glutarate 135g
[0033] 4. Screen print the mixed carbon paste to a surface density of 80g / m 2 , 0.05mmFR4 film, where the screen printing environment temperature is 23℃, the hardness of the ink scraper is 80°, the ink scraper pressure is 40N, the mesh number of the steel wire is 200 mesh, the ink scraper moving speed is 150mm / s, and the ink return knife moving speed is 240mm / s. Finally, the screen-printed carrier is pasted on an 85℃ metal plate for 4 minutes to allow most of the solvent to evaporate, and then heated in a 150℃ oven for 2 hours to obtain a resistive absorbing film. The resistive absorbing film has a high temperature resistance of >180℃, a flat tensile strength of >1.5MPa, a resistance change of 1.0-1.1, and a surface density of 92g / m 2 .like Figure 1 shown.
[0034] The resistive absorbing film is attached to the polyurethane foam or the polymethacrylimide foam to make a composite functional absorbing material or a stealth material.
[0035] Embodiment 2:
[0036] A resistive wave absorbing film is prepared by coating a mixed carbon slurry onto a film carrier and curing the mixed carbon slurry. The raw materials of the mixed carbon slurry are configured according to the mass ratio described in Table 2. The highly conductive carbon black particles selected are CaBOT carbon black VXC-72R.
[0037] The method for preparing the resistive wave absorbing film comprises the following steps:
[0038] 1. Add benzoxazine resin and bisphenol A epoxy resin in a flask in proportion, heat to 70°C, stir evenly to obtain a mixed solution in which the resin is completely dissolved, and then cool to room temperature for use;
[0039] 2. Add the fixed proportion of solvent, anhydride curing agent and additives into the stainless steel can according to the table below, stir and disperse evenly, and use a disperser with a speed of 600-1200r / min to disperse;
[0040] 3. Add the resin mixture prepared in step 1 to the mixture prepared in step 2 according to the ratio in Table 4 below, then add carbon black particles and graphite particles in a fixed ratio, stir at high speed for 3 hours, transfer to a three-roll grinder and grind for 3 times to obtain a mixed carbon slurry for use. The ratio of raw materials added is shown in Table 2:
[0041] Table 2: Raw material ratios of Example 2
[0042] Components Mass Highly conductive carbon black particles (2um) 58g Graphite particles (1.7um) 142g Benzoxazine resin BEP 110g Bisphenol A epoxy resin 310g Methyltetrahydrophthalic anhydride MTHPA 252g 2-Ethyl-4-methylimidazole 2E4MZ 2g BYK-163 (BYK brand) 20g Tributyl phosphate 3g Dimethyl glutarate 103g
[0043] 4. Screen print the mixed carbon paste to a surface density of 81g / m 2 On 0.05mmFR4: The screen printing environment temperature is 23℃, the hardness of the ink scraper is 80°, the ink scraper pressure is 40N, the mesh number of the steel wire is 200 mesh, the ink scraper moving speed is 150mm / s, and the ink return knife moving speed is 240mm / s. Finally, the screen-printed carrier is pasted on an 85℃ metal plate for 4 minutes to allow most of the solvent to evaporate, and then heated in a 150℃ oven for 2 hours to obtain a resistive absorbing film. The high temperature resistance of the resistive absorbing film is greater than 180℃, the flat tensile strength is greater than 1.5MPa, and the resistance value changes from 1.0 to 1.1.
[0044] Embodiment 3:
[0045] A resistive wave absorbing film is prepared by coating a mixed carbon slurry onto a film carrier and curing the mixed carbon slurry. The raw materials of the mixed carbon slurry are configured according to the mass ratio described in Table 3. The highly conductive carbon black particles selected are CaBOT carbon black VXC-72R.
[0046] The method for preparing the resistive wave absorbing film comprises the following steps:
[0047] 1. Add benzoxazine resin and epoxy resin in a flask in proportion, heat to 70°C, stir evenly to obtain a mixed solution in which the resin is completely dissolved, and then cool to room temperature for use;
[0048] 2. Add the fixed proportion of solvent, anhydride curing agent and additives into the stainless steel can according to the table below, stir and disperse evenly, and use a disperser with a speed of 600-1200r / min to disperse;
[0049] 3. Add the resin mixture prepared in step 1 to the mixture prepared in step 2 according to the proportions in Table 3 below, then add carbon black particles and graphite particles in a fixed proportion, stir at high speed for 3 hours, transfer to a three-roll grinder and grind for 3 times to obtain a mixed carbon slurry for use. The proportions of raw materials added are as follows:
[0050] Table 3: Raw material ratios of Example 3
[0051] Components Mass Highly conductive carbon black particles (2um) 58g Graphite particles (1.7um) 142g BEP 110g Bisphenol A epoxy resin 310g Methylhexahydrophthalic anhydride MHHPA 252g 2-Methylimidazole 2MZ 2g BYK-163 (BYK brand) 20g Tributyl phosphate 3g Dimethyl glutarate 103g
[0052] 4. Screen print the mixed carbon paste to a surface density of 80g / m 2 On 0.05mm PI film: the screen printing environment temperature is 23℃, the hardness of the squeegee is 80°, the squeegee pressure is 40N, the mesh number of the steel wire is 200 mesh, the squeegee moving speed is 150mm / s, and the ink return knife moving speed is 240mm / s. Finally, the screen-printed carrier is pasted on an 85℃ metal plate for 4 minutes to allow most of the solvent to evaporate, and then heated in a 150℃ oven for 2 hours to obtain a resistive absorbing film. The high temperature resistance of the resistive absorbing film is greater than 180℃, the flat tensile strength is greater than 1.5MPa, and the resistance value changes from 1.0 to 1.1.
[0053] Comparative Example 1:
[0054] A resistive absorbing film, the preparation method steps and raw material ratios are consistent with those of Example 1, the difference is that in the comparative example, no carbon black is added to the conductive carbon powder, and the conductive carbon powder is all graphite.
[0055] The proportions of the components in Comparative Example 1 are:
[0056] Table 4: Raw material ratios of comparative example 1
[0057]
[0058]
[0059] The tensile strength of the absorbing film in Comparative Example 1 is less than 1.0 MPa. Compared with Example 1, the adhesive performance of the prepared absorbing film is significantly reduced.
[0060] The resistance-type absorbing films of Comparative Example 1 and Examples 1 to 3 were tested for performance, and the test results are as follows:
[0061] Table 5: Performance test of the absorbing films prepared in Examples 1 to 3
[0062]
[0063] Table 6: Reflectivity test of the absorbing films prepared in the embodiments and comparative examples
[0064] Wave absorbing effect L S C X Ku Ka Example 1 -0.45 -2.88 -16.84 -13.74 -10.34 -8.99 Example 2 -0.15 -0.97 -4.90 -4.41 -4.73 -7.37 Example 3 -0.16 -1.09 -5.71 -5.05 -5.52 -7.63 Comparative Example 1 -0.09 -0.13 -1.62 -2.32 -1.64 -2.12
[0065] It can be seen from Tables 5 and 6 that the absorbing film made without adding carbon black has low tensile strength and low reflectivity.
Claims
1. A resistive absorbing film, It is characterized in that It is mainly prepared from a mixed carbon slurry and a film carrier, wherein the mixed carbon slurry comprises the following components by weight: 10 to 15 parts of benzoxazine resin, 25 to 40 parts of epoxy resin, 0.1 to 5 parts of an auxiliary agent, 10 to 15 parts of a solvent, 15 to 35 parts of an anhydride curing agent, and 10 to 35 parts of a conductive powder; The solvent includes one or more of ethylene glycol butyl ether acetate, dimethyl glutarate, and dimethyl succinate; The conductive powder is a mixture of carbon black particles and graphite particles, wherein the carbon black particles are highly conductive carbon black particles with a radius of 0.5 μm to 8 μm; the radius of the graphite particles is 0.5 μm to 5 μm, and the mixing mass ratio of the carbon black particles to the graphite particles is 1:1 to 8.
2. The resistive absorbing film according to claim 1, It is characterized in that The epoxy resin is bisphenol A epoxy resin; the anhydride curing agent includes a combination of one or more of liquid methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, and methylnadic anhydride.
3. The resistive absorbing film according to claim 1, It is characterized in that The auxiliary agent includes a combination of one or more of a dispersant, a defoamer, and a promoter; the dispersant is a BYK polymer wetting dispersant, and the weight portion of the dispersant is 1 to 4 parts; the defoamer is tributyl phosphate, and the weight portion of the defoamer is 0.1 to 0.5 parts; the promoter is an imidazole promoter, and the imidazole promoter includes a combination of one or more of 2-methylimidazole, 2-ethyl-4-methylimidazole, and 2-phenylimidazole, and the weight portion of the promoter is 0.1 to 0.5 parts.
4. The resistive absorbing film according to claim 1, It is characterized in that The film carrier is one of FR4 film and PI film, and the thickness of the film carrier is ≤0.1 mm and the surface density is ≤100 g / m 2 .
5. A method for preparing a resistive absorbing film according to any one of claims 1 to 4, It is characterized in that The following steps are involved: The benzoxazine resin and the epoxy resin are heated and mixed evenly, and after cooling, they are added into a mixed solution of a solvent, anhydride curing agent and an auxiliary agent and mixed evenly, and conductive powder is added to disperse and grind to obtain a mixed carbon slurry, and the mixed carbon slurry is screen-printed on a film carrier and cured to obtain the resistive absorbing film.
6. The preparation method according to claim 5, It is characterized in that The heating and mixing is to maintain the temperature at 65-80° C. for stirring; the cooling is to cool to room temperature; the dispersing is performed by a disperser with a speed of 600-1200 r / min; the grinding is performed by a three-roll grinder for 2-3 times.
7. The preparation method according to claim 5, It is characterized in that The ambient temperature of the silk screen printing is 18-28°C, and the silk screen printing adopts a silk screen printing machine. The parameters of the silk screen printing machine are: the hardness of the scraper is 65-80°, the pressure of the scraper is 40-50N, the silk screen screen is any one of a steel screen screen or a polyester screen screen, and the mesh number is 200-300 meshes; the moving speed of the scraper is 80-200mm / s, and the moving speed of the ink return knife is 240mm / s.
8. The preparation method according to claim 5, It is characterized in that The curing process is: hot stamping at 80-90°C for 3-5 minutes, and then curing at 150-160°C for 0.5-3 hours.
9. Use of the resistive absorbing film according to any one of claims 1 to 4 or the resistive absorbing film prepared by the preparation method according to any one of claims 5 to 8, It is characterized in that The resistive wave-absorbing film is attached to polyurethane foam or polymethacrylimide foam to prepare a composite functional wave-absorbing material.