A process for reforming pre-hydrogenation

By using the first hydrogenation catalyst and the hydroxyl or carboxyl-containing organic matter in the second reactor in the reforming pre-hydrogenation process, combined with the silicon capture catalyst, the problem of difficulty in removing complex silicon content in the existing technology is solved, and the Efficient silicon removal and catalyst stability meet reforming feed quality standards.

CN116064108BActive Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111278935.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-31
Publication Date
2024-10-01
Estimated Expiration
2041-10-31

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively remove the silicon content in oils with complex types of silicon-containing compounds, especially alkylsilane, silanol or silicon ether silicon-containing compounds, and cannot meet the requirements of low sulfur, low nitrogen and low impurities. Whole feed standard.

Method used

A reforming pre-hydrogenation process method is designed. The first hydrogenation catalyst is used in the first reactor to carry out hydrodesulfurization, hydrodesulfurization and hydrodenitrification reactions, and the second reactor is added containing Organic compounds with hydroxyl and/or carboxyl groups are used to help break Si-O or Si-C bonds, and are used with silicon capture catalysts to perform hydrodesiliconization reactions, and the reaction conditions are controlled to achieve efficient removal of silicon content.

Benefits of technology

It achieves effective desilication of oil with high silicon content, ensures the quality of reforming feed, improves the stability and economic benefits of the catalyst, and meets the standard requirements of low sulfur, low nitrogen and low impurities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116064108B_ABST
    Figure CN116064108B_ABST
Patent Text Reader

Abstract

The present invention discloses a process method for reforming pre-hydrogenation, wherein the raw oil and hydrogen enter the first reactor, the first reactor is filled with at least the first hydrogenation catalyst, the removal rate of sulfide in the raw oil in the first reactor is controlled to be 50-90%, the removal rate of nitride is 50-90%, and the removal rate of olefin is 95-100%; the effluent of the first reactor and at least one organic matter containing hydroxyl and / or carboxyl enter the second reactor, the second reactor is filled with at least one silicon-capturing catalyst, the reaction temperature is controlled to be 250-400°C, and the oil product is desiliconized. The process method of the present invention is aimed at the problem that the silicon content in the raw oil is not up to standard, and it is separated from the conventional thinking of the prior art, adopts the idea of ​​first de-olefination, desulfurization and denitrification and then desiliconization, and designs a process line with simple flow, low energy consumption and low cost to obtain qualified reforming feed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of clean oil refining, and in particular relates to a reforming pre-hydrogenation process method. Background Art

[0002] With the oversupply of fuel oil in my country, especially the oversupply of diesel, more and more oil refining enterprises are transforming to the chemical industry. Reforming technology is an important process technology for producing aromatics, and the raw oil for the reforming unit usually needs to be low in sulfur (<0.5ppm), low in nitrogen (<0.5ppm), and low in impurity content (<0.5ppm), mainly from naphtha, coking naphtha, etc. These raw materials need to be hydrotreated to remove impurities.

[0003] CN200710012085.5 discloses a method for hydrofining silicon-containing distillate oil. In this method, silicon-containing distillate oil raw material and hydrogen are passed through at least two hydrofining catalyst beds under hydrofining conditions. The silicon-containing distillate oil raw material first passes through a hydrofining catalyst bed with a silicon-capturing function, and then passes through a conventional hydrofining catalyst bed; wherein the hydrofining catalyst with a silicon-capturing function has a large pore volume and specific surface area and a relatively low metal content. When the raw material passes through the hydrofining catalyst bed with a silicon-capturing function, the reaction conditions are: reaction pressure 1.0-12.0MPa, hydrogen-oil volume ratio 100-2000, volume space velocity 0.5-10.0h -1 , reaction temperature 160~320℃; reaction conditions when the raw material passes through the conventional hydrogenation catalyst bed are: reaction pressure 1.0~12.0MPa, hydrogen-to-oil volume ratio 100~2000, volume space velocity 0.5~5.0h -1 , reaction temperature 200 ~ 420 ° C. When the silicon content is low, and the silicon-containing compounds are mainly cyclosiloxanes, this process condition can meet the desiliconization requirements.

[0004] CN200910188090.0 discloses a coking naphtha silicon scavenger and its application. The coking naphtha silicon scavenger of the invention uses alumina as a carrier, silicon dioxide as an auxiliary agent, and W, Mo and Ni as hydrogenation components. The pore volume of the coking naphtha silicon scavenger is 0.5-0.70 ml / g, and the specific surface area is 250-500 m 2 / g, the content of hydrogenated components in terms of oxides is 1% to 20%, and the acid content is 0.3 to 0.5 mmol / g. The coking naphtha silicon scavenger of the invention can effectively remove the impurity silicon contained in the coking naphtha, and protect the coking naphtha hydrogenation refining catalyst from permanent deactivation caused by silicon poisoning. The reaction conditions for the application of the coking naphtha silicon scavenger in the invention are: reaction pressure 1.0 to 12.0 MPa, hydrogen-to-oil volume ratio 100 to 2000, volume space velocity 1 to 15.0 h -1, reaction temperature 160 ~ 320 ° C. However, the catalyst and process conditions are mainly for cyclosiloxane compounds with good silicon capture performance.

[0005] According to the research on existing technologies, silicon in crude oil products is mainly cyclosiloxanes, which are relatively easy to remove under the existing hydrogenation process conditions, thereby reducing the poisoning of downstream catalysts. However, with the development of oil product development technology, other types of silicon compounds may be introduced into oil products, and there are crude oil products that cannot effectively remove and reduce the silicon content to the standard requirements using the existing reaction process, and new solutions need to be sought. Summary of the invention

[0006] Due to the complex sources of naphtha, some oil products have a silicon content as high as 300-1000ppm, and the current technology generally desiliconizes oil products with a silicon content of less than 100ppm and in the form of epoxysilane. Cyclosiloxanes are easier to remove. The inventors have found through a large number of experimental studies that the silicon in many oil products is difficult to remove. The type of silicon-containing compounds has changed. There are more alkylsilanes, silanols or silyl ethers containing silicon compounds. After the raw oil products are treated according to the desiliconization methods and processes of the prior art, the silicon content is still very high. It is difficult to make the silicon content meet the standard by adjusting the process operating conditions. The technical solution of the present invention is based on the above premise and discovery. In order to solve the above problems, the present invention provides a process method for reforming pre-hydrogenation. For oil products with high silicon content and complex silicon compound types, a process that matches a catalyst and a process flow is designed to produce high-quality reforming feed under the conditions of simple process, low energy consumption and low cost.

[0007] The technical purpose of the present invention is achieved through the following technical solutions:

[0008] A reforming pre-hydrogenation process method comprises the following contents: crude oil and hydrogen enter a first reactor, the first reactor is filled with at least a first hydrogenation catalyst, and the removal rate of sulfide, the removal rate of nitride and the removal rate of olefin in the crude oil in the first reactor are controlled to be 50-90%, 50-90% and 95-100%; the effluent of the first reactor and at least one organic matter containing hydroxyl and / or carboxyl enter a second reactor, the second reactor is filled with at least one silicon-trapping catalyst, the reaction temperature is controlled to be 250-400°C, preferably 250-380°C, and the oil product is desiliconized.

[0009] In the above-mentioned process method of the present invention, the raw oil is at least one of straight-run naphtha, coker naphtha, hydrogenated reformed naphtha, jet fuel, gasoline and light diesel; the silicon content of the raw oil is 1-3000μg / g, and the raw oil with a high silicon content needs to be desiliconized several times to meet the standard. The raw oil with a silicon content of 5-700μg / g is preferably treated. According to the properties of the raw oil, it can be optionally treated by a conventional desiliconization method in the prior art so that it does not contain (or contains below the standard) easily removable silicon compounds such as cyclosiloxanes and silanes, so as to avoid poisoning the catalyst in the first reactor. That is, the raw oil entering the first reactor and contacting with the first hydrogenation catalyst contains at least one silicon-containing compound other than cyclic siloxane compounds and silane compounds. Among them, the cyclic siloxane compound is a cyclic silicon-oxygen bond (-Si-O-) n , n≥3 as the main chain of organic silicon compounds, such as those having the general formula (H 2 SiO) n , n≥3, or a compound in which H in the general formula is replaced by an alkyl group, a halogen, etc.; the silane compound is a compound having Si n H 2n+2 , an organosilicon compound of the general formula: n≥1.

[0010] Furthermore, the silicon-containing compound in the feedstock oil includes but is not limited to at least one of alkylsilane, silanol or silane ether silicon-containing compounds.

[0011] Furthermore, as a specific embodiment, the silicon-containing compounds in the crude oil include but are not limited to at least one of tetramethylsilane, triethylsilane, tetraethylsilane, tetrapropylsilane, trimethylsilanol, dimethoxydimethylsilane, diethoxydimethylsilane, hexamethyldisiloxane, dimethyloctylchlorosilane, octamethyltrisiloxane and n-octyltriethoxysilane.

[0012] The above silicon compounds are more stable than epoxysilane compounds or silane compounds. It is difficult to remove them to meet the requirements using the existing desiliconization conditions and silicon trapping catalysts. The present invention adopts a method of adding organic matter containing hydroxyl and / or carboxyl groups. The inventors found that organic matter containing hydroxyl and / or carboxyl groups helps to remove the above stable silicon compounds. The specific principle may be that the hydroxyl and carboxyl groups in the organic matter help to break the Si-O or Si-C bonds, exposing Si atoms, and then being removed by the silicon trapping agent.

[0013] In the process method of the present invention, hydrodeolefination, hydrodesulfurization and hydrodenitrogenation reactions occur in the first reactor, and hydrodesiliconation, hydrodesulfurization and hydrodenitrogenation reactions are carried out in the second reactor. The depth of hydrodesulfurization, hydrodenitrogenation and hydrodeolefination of the effluent of the first reactor is controlled. Under the process conditions of the first reactor, the silicon-containing compounds in the feed oil are difficult to remove and will not affect the hydrogenation catalyst. The removal rate of the silicon-containing compounds is about 0-1.0%.

[0014] Furthermore, the process conditions of the first reactor are: reaction pressure 1.5-3.0 MPa, hydrogen-oil volume ratio 80-200, volume space velocity 1-5 h -1 , the reaction temperature is 100-250°C, preferably 120-220°C, most preferably 150-220°C;

[0015] Furthermore, the process conditions in the second reactor are: reaction pressure 3.0-8.0 MPa, hydrogen-to-oil volume ratio 200-500, volume space velocity 5-10 h -1 .

[0016] Furthermore, the mass content of the organic matter containing hydroxyl and / or carboxyl groups entering the second reactor in the feedstock oil is 0.01-5wt%, preferably 0.5-3.5wt%, and more preferably 1-2.5wt%.

[0017] Further, the organic matter containing hydroxyl and / or carboxyl groups is alcohol or organic acid, and more preferably C1-C10 alcohol and / or acid, more preferably C2-C8 alcohol and / or acid; most preferably C2-C6 alcohol and / or acid. Wherein, the alcohol and / or acid includes monohydric alcohol, dihydric alcohol, trihydric alcohol, monobasic acid, dibasic acid and tribasic acid; as a more specific embodiment, the organic matter containing hydroxyl and / or carboxyl groups is selected from at least one of ethanol, ethylene glycol, propanol, propylene glycol, glycerol, butanol, butanediol, butanetriol, pentanol, acetic acid, oxalic acid, tartaric acid, succinic acid, glycolic acid and citric acid.

[0018] Furthermore, the organic matter containing hydroxyl and / or carboxyl groups is mixed with the feedstock oil before the reactor or both are introduced into the reactor for online mixing. As one of the preferred technical solutions, the organic matter containing hydroxyl and / or carboxyl groups is mixed with the feedstock oil first and preheated before being introduced into the second reactor, the preheating temperature is 200-350° C., the preheating time is 10 min-2 h, preferably 10 min-30 min.

[0019] Further, according to the fact that the sulfur, nitrogen and silicon contents in the effluent of the second reactor do not meet the standards, the effluent of the second reactor is subjected to the following different treatments:

[0020] When the sulfur content in the second reactor effluent is greater than 0.5 ppm and / or the nitrogen content is greater than 0.5 ppm, the second reactor effluent is recycled to the inlet of the second reactor for further hydrogenation until the second reactor effluent meets the quality requirements of the reforming feed.

[0021] When the sulfur content in the effluent of the second reactor is ≤0.5ppm and the nitrogen content is ≤0.5ppm, but the silicon content is >1ppm, after the effluent of the second reactor is separated, 95-100% of the silicon-containing compounds in the effluent of the second reactor are in the light component, the light component is recycled to the inlet of the second reactor for hydrogenation and desiliconization, and the heavy component is used as reforming feed.

[0022] Furthermore, the light component is the fraction of the second reactor effluent with a temperature less than 70° C.; the heavy component is the fraction of the second reactor effluent with a temperature greater than or equal to 70° C.

[0023] Further, at least the first reactor is filled with a first hydrogenation catalyst, the active metal of the first hydrogenation catalyst is a VIB group metal or / and a VIII group metal, based on the weight of the hydrogenation catalyst, the content of the VIB group metal oxide is 5% to 30%, preferably 15% to 25%, and the content of the VIII group metal oxide is 1% to 15%, preferably 3% to 8%; the carrier is alumina or alumina modified with an additive, and the additive is one or more of B, P, Mg, Zr or Si; based on the weight of the carrier, the additive is 3% to 15% in terms of oxide, preferably 3% to 10%. The preparation method of the catalyst is well known in the art, and one or more of the impregnation method, co-extrusion method, and co-precipitation method can be used. The hydrogenation deolefination reaction is mainly carried out on the first hydrogenation catalyst, which can prevent olefin polymerization and coking, causing poisoning and deactivation of the catalyst, and can remove part of the sulfide and nitride, while the silicon-containing compound will not affect the catalyst in the first reactor.

[0024] Furthermore, according to the properties of the oil product, when the raw oil contains easily removable silicon compounds such as cyclosiloxanes and silanes, the oil product is first treated by a conventional desiliconization method in the prior art, and the method is to add a reactor filled with a conventional silicon capture catalyst at the front end of the first reactor, or in the first reactor, fill a conventional silicon capture catalyst bed upstream of the first hydrogenation catalyst bed, so that the easily removable silicon compounds are removed first. Under the silicon capture process conditions of the prior art, the difficult-to-remove silicon compounds still exist in the oil product and will not be removed in the first reactor. The conventional silicon capture catalyst is well known to those skilled in the art. As one of the specific embodiments, it is a catalyst with Mo-Ni as the active component and alumina as the carrier, wherein the mass content of the active component in terms of oxide is 5% to 10%.

[0025] Furthermore, the second reactor is filled with at least one silicon capture catalyst, the active metal of the silicon capture catalyst is a metal of Group VIB or / and a metal of Group VIII, the carrier is alumina, and the mass content of the metal oxide of Group VIB is 5% to 30%, preferably 5% to 15%, and the mass content of the metal oxide of Group VIII is 1% to 15%, preferably 2% to 6%, based on the weight of the silicon capture catalyst; the specific surface area is 100 to 500 m 2 / g, preferably 300-500m 2 / g, the pore volume is 0.3-1.2mL / g, preferably 0.4-0.8mL / g. The preparation method of the catalyst is well known in the art, and one or more of an impregnation method, a co-extrusion method, and a co-precipitation method can be used. Under the process conditions of the second reactor, under the action of the silicon-capturing catalyst in the second reactor, the silicon-containing compound in the first reaction effluent can be removed and the sulfide and nitride can be further removed.

[0026] Furthermore, as one of the preferred embodiments, a hydrogenation catalyst with desulfurization and denitrification functions is loaded downstream of the silicon capture catalyst bed of the second reactor, preferably the first hydrogenation catalyst is loaded to ensure the removal of residual sulfides and nitrides, and the volume ratio of the silicon capture catalyst to the hydrogenation catalyst is 9:1 to 1:1.

[0027] The process method of the present invention is aimed at the problem of substandard silicon content in the crude oil. It deviates from the conventional thinking of the prior art and adopts the idea of ​​first removing olefins, desulfurizing and denitrogenating, and then desiliconizing, and designs a process line with simple flow, low energy consumption and low cost to obtain qualified reforming feed. Specifically, since the silicon-containing compounds in the crude oil are very stable, through the method of the present invention, the crude oil passes through the first reactor and the second reactor in sequence. In the first reactor, all olefins in the crude oil are removed, and part of the sulfides and nitrides are removed to prevent the olefins from coking in the second reactor and causing carbon deposition poisoning and deactivation of the catalyst. At the same time, the silicon-containing compounds will not cause silicon poisoning of the catalyst in the first reactor, thereby improving the stability of the catalyst; the effluent from the first reactor enters the second reactor, and the silicon-containing compounds are removed under the action of an organic additive containing hydroxyl and / or carboxyl groups, and further undergo hydrodesulfurization and hydrodenitrogenation reactions to generate qualified reforming feed. The silicon compounds in the above oil products are more stable than epoxysilane compounds or silane compounds. It is difficult to remove them to meet the requirements using the desiliconization conditions and silicon-trapping catalysts of the prior art. The present invention adopts a method of adding organic matter containing hydroxyl and / or carboxyl groups. The inventors found that organic matter containing hydroxyl and / or carboxyl groups helps to remove the above stable silicon compounds. The specific principle may be that the hydroxyl and carboxyl groups in the organic matter help to break the Si-O or Si-C bonds, exposing the Si atoms, and then being removed by the silicon-trapping agent. The process method of the present invention can solve the problem of unqualified reforming feed faced by enterprises, creating considerable economic benefits for enterprises.

[0028] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 .Schematic diagram of the reforming pre-hydrogenation process unit used in the example. DETAILED DESCRIPTION

[0030] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0031] The composition of the catalyst provided by the present invention can be characterized by combining inductively coupled plasma ICP and XRF energy spectrum to characterize the total content of the VIB group metal and the total content of the VIII group metal in the catalyst. The specific surface area and pore volume of the catalyst provided by the present invention are analyzed by nitrogen physical adsorption, and the hydroxyl concentration on the catalyst surface is analyzed by infrared acid adsorption. The silicon content and type in the raw oil and the product of the present invention are analyzed by ICP and nuclear magnetic resonance, wherein the silicon content in the raw oil and the product is analyzed by ICP, and then the nuclear magnetic resonance 29Si MAS NMR is used to analyze the silicon type in the raw oil and the product. The silicon content and silicon type deposited on the catalyst provided by the present invention are analyzed by XRF and 29Si MAS NMR, wherein the silicon content deposited on the catalyst is analyzed by XRF, and the silicon type deposited on the catalyst is analyzed by 29Si MAS NMR.

[0032] In Example 1, a silicon capture catalyst was prepared:

[0033] Example 1

[0034] An equal volume of a solution containing nickel salt and molybdenum salt was impregnated into an alumina carrier, then dried at 120°C for 3 h in an air atmosphere, and calcined at 400°C for 3 h to obtain a silicon-trapping catalyst C-1.

[0035] The weight percentages of the components in the silicon trapping catalyst C-1 are: 14.1% molybdenum oxide, 4.5% nickel oxide, and the rest aluminum oxide. The catalyst properties are shown in Table 1.

[0036] In Example 2, a first hydrogenation catalyst was prepared:

[0037] Example 2

[0038] An equal volume of a solution containing nickel salt and molybdenum salt was impregnated into a silicon-modified alumina carrier, then dried at 120° C. for 3 h in an air atmosphere, and calcined at 450° C. for 3 h to obtain a first hydrogenation catalyst C-2.

[0039] The weight percentages of the components in the first hydrogenation catalyst C-2 are: 21.6% molybdenum oxide, 5.8% nickel oxide, and the rest aluminum oxide. The catalyst properties are shown in Table 1.

[0040] Table 1.

[0041] Catalyst No. <![CDATA[Specific surface area, m 2 .g -1 > <![CDATA[Pore volume, ml.g -1 > Average pore size, nm C-1 389 0.65 6.7 C-2 279 0.46 6.6

[0042] by Figure 1Taking the reforming pre-hydrogenation process of the present invention as an example, the raw oil 1 and hydrogen 2 enter the first hydrogenation reactor 3 under certain temperature and pressure conditions, and carry out hydrodesulfurization, hydrodenitrogenation and hydrodeolefination reactions in the first hydrogenation reactor to obtain the first hydrogenation reactor effluent 4. The first hydrogenation reactor effluent 4 enters the upper bed 5 of the second hydrogenation reactor to carry out silicon capture reaction to remove silicon in the first hydrogenation reactor effluent; then enters the lower bed 6 of the second hydrogenation reactor to carry out hydrodesulfurization and hydrodenitrogenation reactions to obtain the second hydrogenation reactor effluent 7.

[0043] The first hydrogenation reactor mainly undergoes hydrodesulfurization, hydrodenitrogenation, and hydrodeolefination reactions to generate a low-sulfur and low-nitrogen naphtha component, namely, the first hydrogenation reactor effluent 4. The upper bed layer 5 of the second hydrogenation reactor mainly undergoes silicon capture reactions to remove silicon from the first hydrogenation reactor effluent to generate a low-sulfur, low-nitrogen, and low-silicon naphtha component; the lower bed layer 6 of the second hydrogenation reactor mainly undergoes hydrodesulfurization and hydrodenitrogenation reactions to remove the remaining sulfides and nitrides to generate a qualified reforming feed, namely, the second hydrogenation reactor effluent 7.

[0044] Example 3

[0045] exist Figure 1 In the reaction device, one catalyst bed is provided in the first hydrogenation reactor, and two catalyst beds are provided in the second hydrogenation reactor. The first hydrogenation reactor is filled with the Ni-Mo type first hydrogenation catalyst C-2 prepared in Example 2, the upper bed 5 of the second hydrogenation reactor is filled with the silicon capture catalyst C-1 prepared in Example 1, and the lower bed 6 of the second hydrogenation reactor is filled with the first hydrogenation catalyst C-2 prepared in Example 2. The volume ratio of the upper bed and the lower bed catalyst in the second hydrogenation reactor is 7:3. The catalyst is first subjected to sulfurization treatment, and the sulfurization conditions are: temperature of 290°C, hydrogen partial pressure of 2.8MPa, hydrogen-to-oil ratio of 500:1, and volume space velocity of 2.0h -1 , sulfurized oil is 3.0% CS 2 The temperature of the reaction bed in each reaction zone during the reaction process is stable and controllable.

[0046] 1.0wt% of succinic acid was added to the effluent of the first hydrogenation reactor. The raw oil was naphtha provided by a refinery of Sinopec. The silicon content of the raw oil was 540μg / g, the sulfur content was 2580μg / g, and the nitrogen content was 467μg / g. The types of silicon in the raw oil were tetramethylsilane, dimethoxydimethylsilane, tetraethylsilane and tetramethylcyclosiloxane according to nuclear magnetic resonance analysis. In order to protect the catalyst in the first reactor, the raw oil was first subjected to conventional desiliconization treatment, using a silicon capture catalyst well known to those skilled in the art, with Mo-Ni as the active component and alumina as the carrier, wherein the mass content of the active component in terms of oxide was 8%. The reaction pressure was 3.0Mpa, the hydrogen-to-oil volume ratio was 100:1, the reaction temperature was 230°C, and the volume space velocity was 6.0h -1 The tetramethylcyclosiloxane was removed under the process conditions of , and the silicon content was 533 μg / g, and then the reaction was carried out in the first reactor. The reaction process conditions and results are shown in Table 2.

[0047] Example 4

[0048] The reaction device, catalyst and sulfurization process used are the same as those in Example 3.

[0049] 1.0wt% ethanol is added to the effluent of the first hydrogenation reactor. The raw oil is naphtha provided by a refinery of Sinopec. The silicon content, sulfur content and nitrogen content of the raw oil are 353μg / g, 2882μg / g and 363μg / g, respectively. Nuclear magnetic resonance analysis shows that the silicon types are tetramethylsilane, triethylsilane, trimethylsilanol and tetramethylcyclosiloxane. In order to protect the catalyst in the first reactor, the raw oil is first subjected to conventional desiliconization treatment. A silicon capture catalyst well known to those skilled in the art is used. The catalyst has Mo-Ni as the active component and alumina as the carrier. The mass content of the active component in terms of oxide is 8%. The reaction pressure is 3.0Mpa, the hydrogen-to-oil volume ratio is 100:1, the reaction temperature is 230°C and the volume space velocity is 6.0h -1 The tetramethylcyclosiloxane was removed under the process conditions of , and the silicon content was 350 μg / g, and then the reaction was carried out in the first reactor. The reaction process conditions and results are shown in Table 2.

[0050] Example 5

[0051] The reaction device, catalyst and sulfurization process used are the same as those in Example 3.

[0052] 1.2 wt% acetic acid is added to the effluent of the first hydrogenation reactor. The raw oil is naphtha provided by a refinery of Sinopec. The silicon content, sulfur content and nitrogen content of the raw oil are 353 μg / g, 2882 μg / g and 363 μg / g, respectively. The types of silicon in the raw oil are tetramethylsilane, triethylsilane, trimethylsilanol and tetramethylcyclosiloxane according to nuclear magnetic resonance analysis. In order to protect the catalyst in the first reactor, the raw oil is first subjected to conventional desiliconization treatment, using a silicon-trapping catalyst well known to those skilled in the art, with Mo-Ni as the active component and alumina as the carrier, wherein the mass content of the active component in terms of oxide is 8%. The raw oil is first subjected to conventional desiliconization treatment, using a silicon-trapping catalyst well known to those skilled in the art, under the conditions of reaction pressure of 3.0 MPa, hydrogen-to-oil volume ratio of 100:1, reaction temperature of 230°C and volume space velocity of 6.0 h -1 The tetramethylcyclosiloxane was removed under the process conditions of , and the silicon content was 350 μg / g, and then the reaction was carried out in the first reactor. The reaction process conditions and results are shown in Table 2.

[0053] Example 6

[0054] The reaction device, catalyst and sulfurization process used are the same as those in Example 3.

[0055] 1.0wt% of propylene glycol was added to the effluent of the first hydrogenation reactor. The feedstock oil was naphtha provided by a refinery of Sinopec. The silicon content in the feedstock oil was 353μg / g, the sulfur content was 2882μg / g, and the nitrogen content was 363μg / g. The types of silicon in the feedstock oil were tetramethylsilane, triethylsilane, trimethylsilanol, and tetramethylcyclosiloxane according to nuclear magnetic resonance analysis. In order to protect the catalyst in the first reactor, the feedstock oil was first subjected to conventional desiliconization treatment, using a silicon-trapping catalyst well known to those skilled in the art, with Mo-Ni as the active component and alumina as the carrier, wherein the mass content of the active component in terms of oxide was 8%. The reaction pressure was 3.0Mpa, the hydrogen-to-oil volume ratio was 100:1, the reaction temperature was 230°C, and the volume space velocity was 6.0h -1 The tetramethylcyclosiloxane was removed under the process conditions of , and the silicon content was 350 μg / g, and then the reaction was carried out in the first reactor. The reaction process conditions and results are shown in Table 2.

[0056] Comparative Example 1

[0057] The reaction device, catalyst and sulfurization process used are the same as those in Example 3.

[0058] No organic acid or alcohol is added to the effluent of the first hydrogenation reactor. The raw oil is naphtha provided by a refinery of Sinopec. The silicon content, sulfur content and nitrogen content of the raw oil are 353 μg / g, 2882 μg / g and 363 μg / g, respectively. The types of silicon in the raw oil are tetramethylsilane, triethylsilane, trimethylsilanol and tetramethylcyclosiloxane according to nuclear magnetic resonance analysis. The above raw oil is first subjected to conventional desiliconization treatment, using a silicon capture catalyst well known to those skilled in the art, at a reaction pressure of 3.0 MPa, a hydrogen-to-oil volume ratio of 100:1, a reaction temperature of 230°C and a volume space velocity of 6.0 h -1 The tetramethylcyclosiloxane was removed under the process conditions of , and then entered the first reactor for reaction. The reaction process conditions and results are shown in Table 2.

[0059] Comparative Example 2

[0060] This comparative example uses two hydrogenation reactors, one catalyst bed is set in the first hydrogenation reactor, and one catalyst bed is set in the second hydrogenation reactor. The first hydrogenation reactor is filled with the silicon capture catalyst C-1 prepared in Example 1, and the second hydrogenation reactor is filled with the first hydrogenation catalyst C-2 prepared in Example 2. The catalysts are first subjected to sulfurization treatment. The sulfurization conditions are: temperature 290°C, hydrogen partial pressure 2.8MPa, hydrogen-to-oil ratio 500:1, volume space velocity 2.0h -1 , sulfurized oil is 3.0% CS 2 of aviation fuel.

[0061] The raw material oil is naphtha provided by a refinery of Sinopec. The silicon content in the raw material oil is 538μg / g, the sulfur content is 2882μg / g, and the nitrogen content is 363μg / g. The silicon types in the raw material oil are tetramethylsilane, triethylsilane, and trimethylsilanol according to nuclear magnetic resonance analysis. The reaction process conditions and results are shown in Table 2.

[0062] Table 2

[0063]

[0064]

[0065] The evaluation results in Table 2 indicate that the reforming pre-hydrogenation process of the present invention can effectively remove silicon from crude oil that is difficult to remove using conventional methods.

Claims

1. A reforming pre-hydrogenation process, comprising the following contents: feedstock oil and hydrogen enter a first reactor, the first reactor is filled with at least a first hydrogenation catalyst, and the removal rate of sulfide, the removal rate of nitride, and the removal rate of olefin in the feedstock oil in the first reactor are controlled to be 50-90%, 50-90%, and 95-100%; the effluent of the first reactor and at least one organic matter containing hydroxyl and / or carboxyl groups enter a second reactor, the second reactor is filled with at least one silicon trapping catalyst, and the reaction temperature is controlled to be 250-400° C. to desiliconize the oil product; in, The silicon-containing compound in the feedstock oil is selected from at least one of tetramethylsilane, triethylsilane, tetraethylsilane, tetrapropylsilane, trimethylsilanol, dimethoxydimethylsilane, diethoxydimethylsilane, hexamethyldisiloxane, dimethyloctylchlorosilane, octamethyltrisiloxane and n-octyltriethoxysilane; the organic matter containing hydroxyl and / or carboxyl groups is selected from at least one of ethanol, ethylene glycol, propanol, propylene glycol, glycerol, butanol, butanediol, butanetriol, amyl alcohol, acetic acid, oxalic acid, tartaric acid, succinic acid, glycolic acid and citric acid; the mass content of the organic matter containing hydroxyl and / or carboxyl groups entering the second reactor in the feedstock oil is 0.01-5wt%; The active metal of the silicon capture catalyst is a metal of Group VIB or / and a metal of Group VIII, the carrier is alumina, and based on the weight of the silicon capture catalyst, the mass content of the metal oxide of Group VIB is 5% to 30%, the mass content of the metal oxide of Group VIII is 1% to 15%, and the specific surface area is 100 to 500 m 2 / g, and the pore volume is 0.3~1.2mL / g.

2. The process according to claim 1, characterized in that: The reaction temperature in the second reactor is controlled at 250-380°C to carry out desiliconization of the oil.

3. The process according to claim 1, characterized in that: The reaction temperature of the first reactor is 100~250℃.

4. The process according to claim 3, characterized in that: The reaction temperature of the first reactor is 120~220℃.

5. The process according to claim 4, characterized in that: The reaction temperature of the first reactor is 150~220℃.

6. The process according to claim 1, characterized in that: The raw oil is at least one of straight-run naphtha, coking naphtha, hydrogenated reformed naphtha, jet fuel, gasoline and light diesel; and the silicon content of the raw oil is 1-3000 μg / g.

7. The process according to claim 3, characterized in that: The reaction pressure of the first reactor is 1.5~3.0MPa, the hydrogen-to-oil volume ratio is 80~200, and the volume space velocity is 1~5h -1 .

8. The process according to claim 1, characterized in that: The reaction pressure of the second reactor is 3.0~8.0MPa, the hydrogen-oil volume ratio is 200~500, and the volume space velocity is 5~10h -1 .

9. The process according to claim 1, characterized in that: The mass content of the organic matter containing hydroxyl and / or carboxyl groups entering the second reactor accounts for 0.5-3.5wt% of the feedstock oil.

10. The process according to claim 9, characterized in that: The mass content of the organic matter containing hydroxyl and / or carboxyl groups entering the second reactor accounts for 1-2.5wt% of the feedstock oil.

11. The process according to claim 1, characterized in that: The organic matter containing hydroxyl and / or carboxyl groups is mixed with the feedstock oil before the reactor or both are introduced into the reactor at the same time for online mixing.

12. The process according to claim 1, characterized in that: According to the sulfur, nitrogen and silicon contents in the effluent of the second reactor, the effluent of the second reactor is treated differently as follows: When the sulfur content in the effluent of the second reactor is greater than 0.5 ppm and / or the nitrogen content is greater than 0.5 ppm, the effluent of the second reactor is circulated to the inlet of the second reactor for further hydrogenation until the effluent of the second reactor meets the quality requirements of the reforming feed; When the sulfur content in the effluent of the second reactor is ≤0.5ppm and the nitrogen content is ≤0.5ppm, but the silicon content is >1ppm, after the effluent of the second reactor is separated, 95-100% of the silicon-containing compounds in the effluent of the second reactor are in the light component, the light component is recycled to the inlet of the second reactor for hydrogenation and desiliconization, and the heavy component is used as reforming feed.

13. The process according to claim 1, characterized in that: The active metal of the first hydrogenation catalyst is a VIB group metal or / and a VIII group metal, and the content of the VIB group metal oxide is 5% to 30% based on the weight of the hydrogenation catalyst, and the content of the VIII group metal oxide is 1% to 15%. The carrier is alumina or alumina modified with an additive, and the additive is one or more of B, P, Mg, Zr or Si; based on the weight of the carrier, the additive is 3% to 15% in terms of oxide.

14. The process according to claim 1, characterized in that: When the raw oil contains easily removable silicon compounds such as cyclosiloxanes and silanes, the oil is first treated by a conventional desiliconization method in the prior art, which includes adding a reactor filled with a conventional silicon-trapping catalyst at the front end of the first reactor, or filling a conventional silicon-trapping catalyst bed in the first reactor upstream of the first hydrogenation catalyst bed, so that the easily removable silicon compounds therein can be removed first.

15. The process according to claim 1, characterized in that: A hydrogenation catalyst with desulfurization and denitrification functions is loaded downstream of the silicon capture catalyst bed of the second reactor, and the volume ratio of the silicon capture catalyst to the hydrogenation catalyst is 9:1~1:1.