A magnesium-doped silicon oxide composite negative electrode material and preparation method thereof
Through the preparation of magnesium-doped silicon oxide composite materials, the four-level buffer structure is constructed using pre-magnesification and etching technology, which solves the problem of volume expansion and resource waste of silicon oxide materials in lithium-ion batteries, and improves cycling stability and Electrical performance reduces the preparation cost.
Patent Information
- Application Number
- CN202310000432.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-03
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-01-03
AI Technical Summary
Silicon oxide, as the negative electrode material of lithium-ion battery, volume expansion during circulation causes the material to crack and powder, affecting its circulation stability and first-time Coulomb efficiency, and at the same time, resource waste and cost are high during the preparation process.
Using the preparation method of magnesium-doped silicon oxide composite negative electrode material, the four-level buffer structure is constructed to alleviate volume expansion and improve electrical performance through low-cost premagnetization, silica coating, CVD carbon coating and HF etching technology. .
The manufacturing cost of silicon oxide materials is significantly reduced, the first Coulomb efficiency and cycling stability are improved, energy consumption is reduced through etching and carbon coating, and the conductivity and electrical properties of the materials are improved.
Smart Images

Figure CN116081632B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a lithium ion battery silicon oxide composite negative electrode material and a preparation method thereof. Background Art
[0002] Silicon-based negative electrode materials generally include single-element nano-silicon and silicon oxide. Single-element silicon has a high theoretical capacity, but its volume expands by up to 300% when lithium ions are embedded. Even if it is coated with various forms of carbon, it will crack and pulverize during the cycle. Although the theoretical capacity of silicon oxide material is not as high as that of single-element silicon, its volume expansion when lithium is embedded is relatively small, and it is currently a silicon-based negative electrode material with great potential for large-scale application.
[0003] Even though the expansion coefficient of silicon oxide is slightly lower than that of elemental silicon, it still reaches 110%, which is much higher than the mainstream graphite negative electrode. In the process of repeated ion insertion and extraction, the material will still crack and pulverize due to the large volume expansion, which greatly affects the cycle stability of silicon oxide materials. In addition, because silicon oxide materials will form irreversible inert substances such as Li2O and Li4SiO4 when they are first inserted with lithium, their initial coulomb efficiency is low, which restricts the commercial application of silicon oxide materials. In addition, in the preparation of silicon oxide negative electrode materials, a large amount of fine powder is generated during the air flow pulverization process, which cannot be effectively utilized, resulting in a huge waste of resources and an increase in preparation costs.
[0004] To this end, we proposed a method to prepare silicon 2 Oxide composite negative electrode materials with high first efficiency and long cycle stability in a low-cost manner. Summary of the invention
[0005] The object of the present invention is to provide a magnesium-doped silicon oxide material to solve the problems existing when the above silicon oxide is used as a negative electrode material for lithium-ion batteries.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a magnesium-doped silicon oxide composite negative electrode material comprises the following steps:
[0008] (1) Weighing silicon oxide fine powder and magnesium metal powder in a certain mass ratio, stirring and mixing them evenly, transferring them to a high-temperature vacuum furnace for sintering, and performing jaw crushing, roller crushing, and air flow milling on the sintered material in sequence to obtain a precursor 1;
[0009] (2) coating the surface of the precursor 1 with a layer of silicon dioxide to obtain the precursor 2;
[0010] (3) placing the precursor 2 in a rotary kiln, introducing a carbon source gas and an inert gas at a certain temperature to perform CVD carbon coating on the precursor 2, thereby obtaining the precursor 3;
[0011] (4) The precursor 3 is etched with a certain concentration and amount of HF solution, filtered, washed to neutrality and then dried to obtain a magnesium-doped silicon dioxide composite material.
[0012] Furthermore, in step (1), the silicon oxide fine powder may be fine powder produced during the air flow pulverization process in the preparation of silicon oxide negative electrode material, and its particle size satisfies 0.5um≤D50≤2um, and the metal magnesium powder particle size satisfies 0.5um≤D50≤2um.
[0013] Furthermore, in step (1), the mass ratio of the magnesium powder to the silicon oxide fine powder is (1-5):(19-28).
[0014] Furthermore, in step (1), the sintering process is to increase the temperature from room temperature to 300°C to 500°C at a heating rate of 3°C / min to 5°C / min, keep it warm for 1h to 3h, then increase the temperature to 950°C to 1100°C at a heating rate of 5°C / min to 8°C / min, keep it warm for 1h to 3h, and finally increase the temperature to 1200°C to 1500°C at a heating rate of 1°C / min to 3°C / min, and keep it warm for 3h to 24h.
[0015] Furthermore, in step (1), the particle size of the precursor 1 after final crushing satisfies 4um≤D50≤8um.
[0016] Furthermore, the method used for coating silicon dioxide in step (2) is: The coating thickness is preferably 50-100 nm.
[0017] Furthermore, in step (3), the carbon source gas is one or more of methane, acetylene, and natural gas.
[0018] The inert gas is one or more of nitrogen, argon, helium and neon.
[0019] The CVD carbon coating temperature is 750°C to 950°C, the holding time is 2h to 5h, the ratio of the volume flow rate of the carbon source gas to the volume flow rate of the inert gas is (1 to 5): (19 to 28), and the total gas flow rate is 0.4L / min-1.5L / min;
[0020] The rotary kiln speed is 0.5r / min~2r / min;
[0021] During the CVD carbon coating process, silicon iodide as the core will undergo disproportionation, partially disproportionating into elemental silicon and amorphous silicon dioxide.
[0022] Further, in step (4), the concentration of the HF solution is 4 mol / L-8 mol / L, the etching time is 0.5 h-2 h, and the mass ratio of the HF solution to the precursor 3 is preferably (1-4): (1-2);
[0023] Furthermore, by controlling the concentration / addition amount / time of the HF solution, the degree of etching can be controlled, and the silicon dioxide coated with the shell, or the silicon dioxide coated with the shell and part of the silicon dioxide generated by differentiation can be selectively etched away.
[0024] Another aspect of the present invention relates to a magnesium-doped silicon oxide composite negative electrode material prepared by the above method. Preferably, the magnesium-doped silicon oxide composite negative electrode material includes an inner core and an outer shell, there is a certain gap between the inner core and the outer shell, the porosity is 40%-55%, too large a porosity will cause the carbon layer to fall off, and too small a porosity will weaken its ability to buffer volume expansion, wherein the inner core (particle size is preferably 4um≤D50≤8um) is a magnesium-doped silicon oxide material with a high silicon content and is porous, the outer shell is an amorphous carbon layer (the thickness of the coated carbon layer is preferably 10-50nm), and the magnesium in the composite negative electrode material mainly exists in the form of Mg, MgO, MgSiO3, Mg2SiO4 or several thereof.
[0025] The present invention also relates to the application of the magnesium-doped silicon oxide composite negative electrode material as a negative electrode material for lithium-ion batteries.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The present invention can use the silicon oxide fine powder produced in the air flow milling process as a raw material to prepare the magnesium-doped silicon oxide composite negative electrode material, which provides a new concept and technical route for the high added value utilization of silicon oxide fine powder and can greatly reduce the manufacturing cost of silicon oxide materials.
[0028] 2. The present invention adopts front-end pre-magnesiation to prepare magnesium-doped silicon oxide composite negative electrode material, and magnesium incorporation can be achieved by one high-temperature sintering. While improving the initial coulombic efficiency, compared with the back-end secondary sintering to achieve pre-magnesiation and pre-lithiation, it can significantly reduce energy consumption and reduce production costs.
[0029] 3. The silicon dioxide composite negative electrode material prepared by the present invention adopts a four-level buffer structure to alleviate its volume expansion during the charge and discharge process, and provide support for the long-cycle stability of the material: first, the introduction of inert material matrices such as MgO and MgSiO3 by magnesium doping can play a certain role in buffering volume expansion; second, a micron-scale pore structure is constructed by etching away part of the silicon dioxide produced by the disproportionation of the inner silicon dioxide, which shortens the lithium ion transmission path while absorbing the stress generated by the volume expansion; third, by etching the outer layer of silicon dioxide, a gap is constructed between the inner silicon dioxide matrix and the outer shell carbon layer, further reserving space for volume expansion; fourth, the outermost carbon layer not only limits the expansion of the silicon dioxide matrix, but also improves the conductivity of the material, further improving the electrical properties of the material.
[0030] 4. Disproportionation is carried out while CVD carbon coating is being carried out. Compared with separate sintering, disproportionation reduces one sintering process, reduces energy consumption, controls the increase of silicon grain size, and effectively alleviates volume expansion.
[0031] 5. By etching away part of the silicon dioxide produced during the disproportionation process, the silicon content in the silicon oxide matrix can be increased, further improving its reversible capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Attached Figure 1 This is the XRD spectrum of magnesium-doped silicon dioxide in Example 1. XRD shows a diffraction peak of MgSiO3, indicating that Mg has been successfully incorporated into the silicon dioxide bulk phase. DETAILED DESCRIPTION
[0033] In order to better understand the technical solutions involved in the present invention, the technical solutions of the present invention will be described in detail in the following by way of specific embodiments.
[0034] Example 1
[0035] The preparation method of the magnesium-doped silicon oxide composite negative electrode material comprises the following steps:
[0036] (1) Pre-magnesiation: 900g of silicon oxide fine powder (D50=0.8um) and 100g of magnesium powder (D50=1.3um) produced during the airflow milling process were weighed, mixed evenly and placed in a high-temperature vacuum furnace. The temperature was raised from room temperature to 400°C at a heating rate of 3°C / min, kept at that temperature for 1h, then raised to 950°C at a heating rate of 5°C / min, kept at that temperature for 1.5h, and finally raised to 1350°C at a heating rate of 1°C / min, kept at that temperature for 5h. The collected samples were subjected to jaw crushing, roller crushing and airflow milling, and the final precursor 1 had a D50 of 4.9um and a magnesium content of 9.6%.
[0037] (2) Silica coating: using The precursor 1 was coated with silica by the following method: 800 g of the precursor 1 was stirred and dispersed in a mixed solution of 5 L of ethanol and water in a ratio of 4:1, the pH was adjusted to 9-10 with aqueous ammonia (28%), 500 mL of TEOS was added, the reaction was carried out at room temperature for 6 h, and then the reaction was centrifuged, washed to neutrality, and vacuum dried at -50°C for 24 h to obtain the precursor 2.
[0038] (3) Silicon dioxide carbon coating and disproportionation: 500 g of precursor 2 was placed in a rotary kiln at a speed of 0.5 r / min. Methane was used as the carbon source gas and nitrogen was used as the inert gas protective atmosphere. The total gas flow rate was 0.5 L / min, wherein the acetylene flow rate: nitrogen flow rate was 1:8. The temperature was raised to 900°C at a rate of 5°C / min and kept at that temperature for 3 h to obtain precursor 3, wherein the carbon content of precursor 3 was 2.8%.
[0039] (4) HF etching pore formation: The obtained precursor 3 was added to 2L of 8 mol / L hydrofluoric acid solution and treated for 1 hour. The mixture was filtered and rinsed with ethanol aqueous solution until neutral, and dried to obtain a magnesium-doped silicon dioxide composite material with a core-shell buffer structure.
[0040] Example 2
[0041] (1) Pre-magnesiation: 950 g of silicon oxide fine powder (D50 = 0.8 um) and 50 g of magnesium powder (D50 = 1.3 um) produced during the airflow milling process were weighed, mixed evenly and placed in a high-temperature vacuum furnace. The temperature was raised from room temperature to 400°C at a heating rate of 3°C / min, kept warm for 2 h, then raised to 950°C at a heating rate of 5°C / min, kept warm for 1.5 h, and finally raised to 1450°C at a heating rate of 1°C / min, kept warm for 5 h. The collected samples were subjected to jaw crushing, roller crushing and airflow milling, and the final precursor 1 had a D50 of 5.8 um and a magnesium content of 4.7%.
[0042] (2) Silica coating: using The precursor 1 was coated with silica by the following method: 800 g of the precursor 1 was dispersed in a 5 L mixed solution of ethanol and water in a ratio of 4:1, the pH was adjusted to 9-10 with aqueous ammonia (28%), 400 mL of TEOS was added, the reaction was carried out at room temperature for 6 h, and then the reaction was centrifuged, washed until neutral, and vacuum dried at -50 °C for 24 h to obtain the precursor 2.
[0043] (3) Silicon dioxide carbon coating and disproportionation: 500 g of precursor 2 was placed in a rotary kiln at a speed of 1 r / min. Acetylene was used as the carbon source gas and nitrogen was used as the inert gas protective atmosphere. The total gas flow rate was 0.5 L / min, wherein the acetylene flow rate: nitrogen flow rate was 1:10. The temperature was raised to 900°C at a rate of 5°C / min and kept at that temperature for 3 h to obtain precursor 3, wherein the carbon content of precursor 3 was 2.6%.
[0044] (4) HF etching pore formation: The obtained precursor 3 was added into 2L of 6 mol / L hydrofluoric acid solution and treated for 2h, filtered and rinsed with ethanol aqueous solution until neutral, and dried to obtain a magnesium-doped silicon dioxide composite material with a core-shell buffer structure.
[0045] Example 3
[0046] (1) Pre-magnesiation: 950 g of silicon oxide fine powder (D50 = 0.8 um) and 50 g of magnesium powder (D50 = 1 um) produced during the airflow milling process were weighed, mixed evenly and placed in a high-temperature vacuum furnace. The temperature was raised from room temperature to 400°C at a rate of 3°C / min, kept at that temperature for 1 hour, then raised to 950°C at a rate of 5°C / min, kept at that temperature for 1.5 hours, and finally raised to 1300°C at a rate of 1°C / min, kept at that temperature for 6 hours. The collected samples were subjected to jaw crushing, roller crushing and airflow milling, and the final precursor 1 had a D50 of 5.1 um and a magnesium content of 4.8%.
[0047] (2) Silica coating: using The precursor 1 was coated with silica by the method. 800 g of the precursor 1 was stirred and dispersed in a mixed solution of 5 L of ethanol and water in a ratio of 4:1. Ammonia water (28%) was added to adjust the pH to 9-10. 600 mL of TEOS was added. After reacting at room temperature for 6 hours, the product was centrifuged, washed until neutral, and vacuum dried at -50°C for 24 hours to obtain the precursor 2.
[0048] (3) Silicon dioxide carbon coating and disproportionation: 500 g of precursor 2 was placed in a rotary kiln at a speed of 1 r / min. Acetylene was used as the carbon source gas and nitrogen was used as the inert gas protective atmosphere. The total gas flow rate was 0.5 L / min, wherein the methane flow rate: nitrogen flow rate was 1:10. The temperature was raised to 900°C at a rate of 5°C / min and kept at that temperature for 5 h to obtain precursor 3, wherein the carbon content of precursor 3 was 3%.
[0049] (4) HF etching pore formation: The obtained precursor 3 was added to 1L of 5 mol / L hydrofluoric acid solution and treated for 30 min. The mixture was filtered and rinsed with ethanol aqueous solution until neutral, and dried to obtain a magnesium-doped silicon dioxide composite material with a core-shell buffer structure.
[0050] Comparative Example 1
[0051] (1): 1000g of silicon oxide fine powder (D50 = 0.8um) produced during airflow pulverization was weighed and placed in a high-temperature vacuum furnace. The temperature was raised from room temperature to 400°C at a heating rate of 3°C / min, and kept at that temperature for 1h. The temperature was then raised to 950°C at a heating rate of 5°C / min, and kept at that temperature for 1.5h. Finally, the temperature was raised to 1350°C at a heating rate of 1°C / min, and kept at that temperature for 5h. The collected samples were subjected to jaw crushing, roller crushing and airflow pulverization, and the final precursor 1 had a D50 of 5um and a magnesium content of 0%.
[0052] (2) Silica coating: using The precursor 1 was coated with silica by the method. 800 g of the precursor 1 was stirred and dispersed in a mixed solution of 5 L of ethanol and water in a ratio of 4:1. The pH was adjusted to 9-10 with ammonia water (28%). 500 mL of TEOS was added. After reacting at room temperature for 6 hours, the product was centrifuged, washed until neutral, and vacuum dried at -50°C for 24 hours to obtain the precursor 2.
[0053] (3) Silicon dioxide carbon coating and disproportionation: 500 g of precursor 2 was placed in a rotary kiln at a speed of 1 r / min. Acetylene was used as the carbon source gas and nitrogen was used as the inert gas protective atmosphere. The total gas flow rate was 0.5 L / min, wherein the acetylene flow rate: nitrogen flow rate was 1:10. The temperature was raised to 900°C at a rate of 5°C / min and kept at that temperature for 3 h to obtain precursor 3, wherein the carbon content of precursor 3 was 2.7%.
[0054] (4) HF etching pore formation: The obtained precursor 3 was added to 1L of 5 mol / L hydrofluoric acid solution and treated for 30 min. The mixture was filtered and rinsed with ethanol aqueous solution until neutral, and dried to obtain a magnesium-doped silicon dioxide composite material with a core-shell buffer structure.
[0055] Comparative Example 2
[0056] (1): 900g of silicon oxide fine powder (D50=0.8um) and 100g of magnesium powder (D50=1.3um) produced during the airflow milling process were weighed, mixed evenly and loaded into a high-temperature vacuum furnace, and the temperature was raised from room temperature to 400°C at a heating rate of 3°C / min, kept warm for 1h, then raised to 950°C at a heating rate of 5°C / min, kept warm for 1.5h, and finally raised to 1350°C at a heating rate of 1°C / min, kept warm for 5h. The collected samples were subjected to jaw crushing, roller crushing and airflow milling, and the final precursor 1 had a D50 of 5um and a magnesium content of 9.5%.
[0057] (2) Carbon coating and disproportionation of silicon dioxide: 800 g of precursor 1 was placed in a rotary kiln at a speed of 1 r / min. Acetylene was used as the carbon source gas and nitrogen was used as the inert gas protective atmosphere. The total gas flow rate was 0.5 L / min, where the acetylene flow rate: nitrogen flow rate was 1:10. The temperature was raised to 900°C at a rate of 5°C / min and kept at this temperature for 3 h to obtain a magnesium-doped silicon dioxide material with a carbon content of 2.8%.
[0058] Comparative Example 3
[0059] Carbon coating and disproportionation of silicon oxide: 1000g of silicon oxide fine powder (D50=0.8um) was placed in a rotary kiln with a rotation speed of 1r / min. Acetylene was used as the carbon source gas and nitrogen was used as the inert gas protective atmosphere. The total gas flow rate was 0.5L / min, wherein the acetylene flow rate: nitrogen flow rate was 1:10. The temperature was raised to 900°C at a rate of 5°C / min and kept warm for 3h to obtain carbon-coated silicon oxide fine powder with a carbon content of 2.9%.
[0060] The relevant physical and chemical indicators and electrical performance test results of the above examples and comparative examples are shown in the following table:
[0061] The XRD spectrum was measured by an X-ray diffraction analyzer, the carbon content was measured by a carbon-sulfur analyzer, and the Mg content was measured by ICP.
[0062] Test method: The silicon-based negative electrode materials for lithium-ion batteries prepared in Examples 1-3 and Comparative Examples 1-3 were tested using the following method:
[0063] The electrochemical cycling performance was tested using the following method:
[0064] According to the negative electrode active material: sodium carboxymethyl cellulose (CMC): conductive carbon black (SP): styrene-butadiene rubber (SBR) is mixed in a mass ratio of 94.5:1.5:1.5:2.5 to prepare the working electrode, coated on the copper foil current collector, vacuum dried, and the negative electrode plate is obtained; then the button half-cell is assembled, the electrode is a lithium sheet, the electrolyte is a 1 mol / L LiPF6 mixed with a solvent of EC:DMC:EMC=1:1:1 (v / v), and the separator is Celgard2400. The charge and discharge test of the button battery is carried out on the LAND battery test system of Wuhan Jinnuo Electronics Co., Ltd. The charge and discharge voltage is limited to 0.05~1.5V. The first charge and discharge performance test is carried out at room temperature, 0.1C constant current charge and discharge, and after 10 cycles, it is switched to 0.5C constant current charge and discharge, and the cycle is 100 cycles. The capacity retention rate is calculated. The test results are shown in the following table:
[0065]
[0066] By comparing the data of the above comparative examples and embodiments, it can be found that: after the silicon content of the silicon oxide substrate is increased by doping with magnesium, constructing a core-shell structure and etching part of the silicon dioxide produced by disproportionation, under better conditions, its reversible capacity can reach 1478 mAh / g, the first efficiency is also increased to 85%, and the capacity retention rate after 100 cycles at 0.5c can also reach 93%; in contrast, for comparative examples 1, 2 and 3, without doping with magnesium or constructing a core-shell structure and without increasing the silicon content, its reversible capacity, first efficiency and capacity retention rate are not satisfactory.
[0067] It should be noted that the embodiments described herein are only partial embodiments of the present invention, rather than all implementations of the present invention, and the embodiments are only exemplary, and their role is only to provide a more intuitive and clear way to understand the content of the present invention, rather than to limit the technical solutions described in the present invention. Without departing from the concept of the present invention, all other implementation methods that can be thought of by ordinary technicians in this field without creative work, and other simple replacements and various changes to the technical solutions of the present invention, all belong to the protection scope of the present invention.
Claims
1. A method for preparing a magnesium-doped silicon dioxide composite material, comprising the following steps: (1) Weighing silicon oxide fine powder and magnesium metal powder in a certain mass ratio, mixing them evenly, sintering at high temperature, and crushing the sintered material to obtain a precursor 1; (2) coating the surface of the precursor 1 with a layer of silicon dioxide to obtain the precursor 2; (3) introducing a carbon source gas and an inert gas into the precursor 2 at a certain temperature to perform CVD carbon coating on the precursor 2 to obtain the precursor 3; (4) The precursor 3 is etched with a certain concentration and a certain amount of HF solution, filtered, washed to neutrality and then dried to obtain a magnesium-doped silicon dioxide composite material.
2. The method according to claim 1, wherein: In step (1), the particle size of the silicon oxide fine powder satisfies 0.5um≤D50≤2um, and the particle size of the magnesium powder satisfies 0.5um≤D50≤2um; Furthermore, the mass ratio of the magnesium powder to the silicon oxide fine powder is (1-5):(19-28).
3. The method according to claim 1 or 2, wherein: In step (1), the sintering process is: heating from room temperature to 300°C to 500°C at a heating rate of 3°C / min to 5°C / min, keeping warm for 1h to 3h, then heating to 950°C to 1100°C at a heating rate of 5°C / min to 8°C / min, keeping warm for 1h to 3h, and finally heating to 1200°C to 1500°C at a heating rate of 1°C / min to 3°C / min, keeping warm for 3h to 24h.
4. The method according to any one of claims 1 to 2, wherein: In step (1), the particle size of the precursor 1 satisfies 4um≤D50≤8um.
5. The method according to claim 1, wherein: In step (3), the carbon source gas is one or more of methane, acetylene, and natural gas. The inert gas is one or more of nitrogen, argon, helium and neon.
6. The method according to claim 5, wherein: In step (3), the volume flow rate ratio of the carbon source gas to the inert gas is (1-5):(19-28), and the total gas flow rate is 0.4 L / min-1.5 L / min.
7. The method according to any one of claims 1, 5-6, wherein: In step (3), the CVD carbon coating temperature is 750°C to 950°C, and the insulation time is 2h to 5h.
8. The method according to claim 1, wherein: In step (4), the concentration of the HF solution is 4 mol / L-8 mol / L, and the etching time is 0.5 h-2 h.
9. The method according to claim 8, wherein: In step (4), the mass ratio of the HF solution to the mass ratio of the precursor 3 is (1-4): (1-2).
10. A magnesium-doped silicon dioxide composite material prepared according to the method according to any one of claims 1 to 9.