Asbestos tailings refined magnesium sulfate solution and method and application thereof
By combining high-temperature roasting with additives of ammonium sulfate or ammonium bisulfate, the separation problem of magnesium ions and iron ions in asbestos tailings was solved, the leaching rate of magnesium ions was improved and the leaching rate of iron ions was reduced, and asbestos was realized Efficient utilization of tailings resources and environmental protection.
Patent Information
- Application Number
- CN202310081770.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-01-19
AI Technical Summary
In the existing technology of resource utilization of asbestos tailings, it is difficult to effectively separate magnesium ions and iron ions, resulting in low magnesium ions leaching rate and secondary pollution problems.
The asbestos tailings are mixed with ammonium sulfate or ammonium bisulfate as reaction aids to form insoluble hematite. Magnesium ions enter the leachate, iron ions are enriched in the filter residue, and ammonia is collected through ammonia water. Recycling to achieve the refining of magnesium sulfate solution.
The leaching rate of magnesium ions is improved to reach more than 77%, and the leaching rate of ferrous ions is reduced to below 0.8%, achieving effective separation of magnesium ions and iron ions, and the process is environmentally friendly, with resource utilization and environmental protection significance.
Smart Images

Figure CN116081659B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste extraction, and in particular relates to an asbestos tailings refined magnesium sulfate solution and a method and application thereof. Background Art
[0002] Asbestos mineral resources are abundant, but the grade of asbestos ore is low. A large amount of asbestos tailings will be produced during the production process, resulting in a large amount of asbestos tailings accumulation. The accumulation of asbestos tailings not only causes a waste of mineral resources, occupies land resources, but also has an adverse impact on the surrounding environment and the health of residents.
[0003] At present, the resource utilization technology of asbestos tailings can be roughly divided into two categories: acid leaching and roasting. In the former, the iron, aluminum, calcium and other ions in the acid leaching solution are not fully utilized, resulting in secondary pollution; in the latter, the extraction effect is not good and it is difficult to achieve effective separation. The mixed roasting of asbestos tailings with additives to extract magnesium oxide is a new process for extracting valuable components from asbestos tailings in recent years. However, when asbestos tailings are leached in water, in addition to magnesium ions, metal impurities such as iron ions are also easily leached. The existing treatment methods often have shortcomings such as the need for a separate iron removal step or difficulty in operation. Summary of the invention
[0004] The object of the present invention is to solve at least one of the above-mentioned deficiencies in the prior art. For example, one of the objects of the present invention is to provide a method for refining magnesium sulfate solution from asbestos tailings. Another object of the present invention is to provide a magnesium sulfate solution and ammonia water. Another object of the present invention is to provide an application method of magnesium sulfate solution.
[0005] In order to achieve the above-mentioned object, one aspect of the present invention provides a method for refining magnesium sulfate solution from asbestos tailings, which comprises the following steps: uniformly mixing asbestos tailings powder and a reaction aid, placing the mixture in a high-temperature roasting furnace for roasting treatment, and obtaining a roasting reaction product and gas collected at an exhaust end of the high-temperature roasting furnace; leaching and filtering the roasting reaction product in a reactor, and obtaining a refined magnesium sulfate solution by the filtrate. Among them, the reaction aid includes ammonium sulfate powder and / or ammonium bisulfate powder; the molar ratio of the reaction aid to the asbestos tailings powder is 0.75-1.50:1; the asbestos tailings, measured by mass percentage, include 37.0%-42.0% SiO2, 36.0%-42.0% MgO, 0.8%-1.2% Al2O3, 3.0%-8.0% TFe2O3 and 0.4%-0.7% CaO, and the loss on ignition is 12.0%-13.5%; the mineral types of the roasting reaction product are mainly magnesium sulfate and magnesium sulfate hexahydrate, and also include hematite, forsterite, unreacted serpentine and quartz.
[0006] In an exemplary embodiment of the present invention, the gas collected from the exhaust end of the high-temperature roasting furnace can be absorbed by water to obtain ammonia water.
[0007] In an exemplary embodiment of the present invention, the preparation of the ammonium sulfate powder may include the following steps: adding ammonia water to a refined magnesium sulfate solution, introducing CO2 to neutralize it and heating to precipitate, filtering, and drying the filter residue to obtain basic magnesium carbonate powder, the filtered filtrate is an ammonium sulfate solution, and the ammonium sulfate solution is evaporated and crystallized to obtain ammonium sulfate powder.
[0008] In an exemplary embodiment of the present invention, the leaching rate of Mg ions in the asbestos tailings powder may be 77-97%, and the leaching rate of Fe ions may be 0.03-0.80%.
[0009] In an exemplary embodiment of the present invention, the concentration of Mg ions in the refined magnesium sulfate solution may be 5.67 to 12.25 g / L, and the concentration of Fe ions may be 0.32 to 2.30 mg / L.
[0010] In an exemplary embodiment of the present invention, the calcination temperature may be 650-750° C., and the calcination time may be 60-120 min.
[0011] In an exemplary embodiment of the present invention, the leaching step further comprises: adding a dilute sulfuric acid solution with a pH value of 5 to 6.8 to the roasting reaction product in a reactor, and reacting for 30 to 90 minutes at 25 to 50° C. and a liquid-to-solid ratio of 8 to 20 ml / g.
[0012] In an exemplary embodiment of the present invention, the absorption may include a spraying method and / or a bubbling method.
[0013] Another aspect of the present invention provides a magnesium sulfate solution and ammonia water, wherein the magnesium sulfate solution and ammonia water are obtained by the above-mentioned method for refining magnesium sulfate solution from asbestos tailings.
[0014] Another aspect of the present invention provides an application method of a magnesium sulfate solution, which comprises the following steps: using the above-mentioned refined magnesium sulfate solution; directly evaporating and crystallizing the refined magnesium sulfate solution to obtain refined magnesium sulfate; or adding ammonia water to the refined magnesium sulfate solution for neutralization and precipitation, filtering, and drying the filter residue to obtain magnesium hydroxide powder; or adding ammonia water to the refined magnesium sulfate solution, passing CO2 to neutralize and heat to precipitate, filtering, and drying the filter residue to obtain basic magnesium carbonate powder, the filtered filtrate is an ammonium sulfate solution, and the ammonium sulfate solution is evaporated and crystallized to obtain ammonium sulfate powder.
[0015] Compared with the prior art, the beneficial effects of the present invention may include at least one of the following:
[0016] 1) The present invention allows the additive to react with the iron ions in the asbestos tailings to generate insoluble hematite, and the magnesium ions enter the leaching solution. The iron is enriched in the filter residue in the form of hematite, which can not only improve the leaching rate of magnesium ions, but also achieve the purpose of separating iron and magnesium ions;
[0017] 2) In the present invention, a gas collecting device is connected to the end of the high-temperature roasting furnace to collect the ammonia gas generated during the process, and the obtained ammonia water can be used for the subsequent preparation of magnesium series powder compounds;
[0018] 3) The refined magnesium sulfate solution of the present invention is used to prepare basic magnesium carbonate powder and ammonium sulfate filtrate, and the ammonium sulfate filtrate can be recycled after evaporation and crystallization, thus realizing a green cycle of the process;
[0019] 4) Mg in the refined magnesium sulfate solution of the present invention 2+ The leaching rate of ions is above 77%, the highest can reach 97%, and the leaching rate of Fe ions is below 0.80%, the lowest can reach 0.03%;
[0020] 5) The present invention uses asbestos tailings mainly containing serpentine mixed with auxiliary agent roasting products to perform leaching to extract magnesium components and separate iron components from silicon dioxide residues. A refined magnesium sulfate solution is obtained by one-step leaching, which can be used to prepare a series of magnesium-containing compound products. The silicon dioxide residue can be used to prepare a series of silicon-containing compound products, thereby realizing the resource utilization of solid wastes, which has important significance for resource and environmental protection and ecological and sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The above and other objects and / or features of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which:
[0022] Figure 1 shows XRD patterns of calcination reaction products at different temperatures of the first exemplary embodiment of the present invention;
[0023] Figure 2 The XRD patterns of the calcination reaction product and the water-leached residue of Example 1 of the present invention are shown. DETAILED DESCRIPTION
[0024] Hereinafter, an asbestos tailings refined magnesium sulfate solution and a method and application thereof of the present invention will be described in detail in conjunction with the accompanying drawings and exemplary embodiments.
[0025] First Exemplary Embodiment
[0026] In a first exemplary embodiment of the present invention, a method for refining magnesium sulfate solution from asbestos tailings is provided, the method for refining magnesium sulfate solution from asbestos tailings comprising the following steps:
[0027] S1. Evenly mix the asbestos tailing powder and the reaction aid, and place them in a high-temperature roasting furnace for roasting treatment to obtain a roasting reaction product and gas collected at the exhaust end of the high-temperature roasting furnace.
[0028] Among them, the asbestos tailings, measured by mass percentage, include 37.0% to 42.0% SiO2, 36.0% to 42.0% MgO, 0.8% to 1.2% Al2O3, 3.0% to 8.0% TFe2O3 and 0.4% to 0.7% CaO, and the loss on ignition is 12.0% to 13.5%. The asbestos tailings are mainly serpentine, containing a small amount of talc, quartz, magnetite, brucite and chlorite.
[0029] Wherein, the reaction aid may include ammonium sulfate powder and / or ammonium bisulfate powder. Here, the preparation of ammonium sulfate powder may include the following steps: adding ammonia water to a refined magnesium sulfate solution, introducing CO2 to neutralize and heat to precipitate, filtering, and drying the filter residue to obtain basic magnesium carbonate powder, the filtered filtrate is an ammonium sulfate solution, the ammonium sulfate solution is evaporated and crystallized to obtain ammonium sulfate powder, and the ammonium sulfate powder is used as a reaction aid in step S1 to achieve recycling of the aid and green processing technology.
[0030] Optionally, the molar ratio of the reaction aid to the asbestos tailing powder can be 0.75-1.50:1, where the molar ratio of the aid to the asbestos tailing powder is calculated according to the molar ratio of sulfate ions in the reaction aid to magnesium ions in the asbestos tailings, for example, 0.75, 1.0, 1.25, 1.5. When too much additive is added, it will not only cause a waste of resources, but also increase the leaching rate of iron ions; when too little additive is added, the structural destruction degree of serpentine in the asbestos tailings at the same temperature will be reduced, and the leaching rate of magnesium ions will be low.
[0031] Optionally, the temperature of the roasting treatment may be 650-750°C, and the time of the roasting treatment may be 60-120 minutes. For example, the temperature may be 650°C, 700°C, 750°C, and the time may be 60 minutes, 80 minutes, 90 minutes, 100 minutes, 120 minutes. When the roasting temperature is too low, ammonium sulfate reacts with iron ions in asbestos tailings to form iron sulfate, which increases the leaching rate of iron ions; when the roasting temperature is too high, not only will serpentine be converted into forsterite to reduce the leaching rate of magnesium ions, but also energy will be wasted. When the roasting time is too short, the reaction between the additive and the serpentine in the asbestos tailings will be incomplete, reducing the extraction rate of magnesium ions; if the roasting time is too long, the energy consumption will increase, which is not economical enough.
[0032] Optionally, the mineral types of the roasting reaction product can be mainly magnesium sulfate and magnesium sulfate hexahydrate, and can also include hematite, forsterite, unreacted serpentine and quartz. Here, serpentine and quartz are unreacted products, and serpentine is converted to forsterite at high temperature. Here, the additive reacts with the iron ions in the asbestos tailings to generate insoluble hematite, and finally the magnesium ions enter the leachate, and the iron is enriched in the filter residue in the form of hematite, which can not only improve the leaching rate of magnesium ions, but also achieve the purpose of separating iron and magnesium ions.
[0033] Figure 1 The XRD patterns of the calcination reaction products at different temperatures of the first exemplary embodiment of the present invention are shown, as shown in FIG. Figure 1 As shown, line a is 120 min at 700°C, line b is 120 min at 650°C, line c is 120 min at 600°C, line d is 120 min at 550°C, and line e is 120 min at 500°C, wherein the molar ratio of the reaction aid to the asbestos tailings powder is 0.75-1.50:1.
[0034] S2. Leaching and filtering the roasting reaction product in a reactor to obtain filter residue and filtrate, wherein the filtrate is a refined magnesium sulfate solution.
[0035] Specifically, the roasting reaction product is placed in a reactor containing a leaching solution and equipped with a stirring and heating device for leaching. After the leaching is completed, the leached product is filtered to obtain a filter residue and a filtrate, and the filtrate is a refined magnesium sulfate solution. Optionally, the filtration includes one or more of pressure filtration, gravity filtration, and centrifugal filtration. The purpose of the filtration is to separate the soluble substances and insoluble substances at the end of the reaction. The magnesium sulfate and refined magnesium sulfate obtained by the reaction are both soluble substances that will enter the filtrate, while insoluble substances such as hematite and silica will remain in the filter residue, thereby achieving the purpose of selective leaching.
[0036] Optionally, the leaching step may include: adding a dilute sulfuric acid solution with a pH value of 5 to 6.8 to the roasting reaction product in a reactor, and reacting for 30 to 90 minutes at 25 to 50°C and a liquid-to-solid ratio of 8 to 20 ml / g. For example, the pH value may be 5.5 or 6. Here, the addition of a dilute sulfuric acid solution with a pH value of 5 to 6.8 increases the leaching rate of magnesium ions, and the leaching of iron ions is mainly achieved by roasting and converting it into hematite. At the same time, too low a pH value will lead to an increase in the leaching rate of iron ions. Among them, a pH value of 6.8 is approximately equivalent to directly adding water to react without adjusting the pH.
[0037] Optionally, the liquid-to-solid ratio may be 8 ml / g, 10 ml / g, 12 ml / g, 14 ml / g, and the temperature may be 30°C, 40°C, 45°C. A liquid-to-solid ratio that is too small will result in a low magnesium ion leaching rate, and a liquid-to-solid ratio that is too large will result in a low reaction rate and an increased reaction time. The reaction time may be 40 min, 50 min, or 60 min. Too low a temperature will result in an insufficient reaction and a low magnesium ion leaching rate. Too short a reaction time will result in an incomplete reaction, and too long a reaction time will increase the time cost.
[0038] Optionally, the MgO and TFe2O3 contents in the filtrate are converted based on the MgO and TFe2O3 contents in the asbestos tailings powder, wherein the leaching rate of Mg ions can be 77-97%, and the leaching rate of Fe ions can be 0.03-0.80%. The concentration of Mg ions in the refined magnesium sulfate solution can be 5.67-12.25 g / L, and the concentration of Fe ions can be 0.32-2.30 mg / L.
[0039] Optionally, the filter residue may mainly include silicon dioxide residue, and also include a small amount of hematite, forsterite and unreacted serpentine, which can be used to prepare silicon-containing series compound products.
[0040] In this example, the gas collected from the exhaust end of the high-temperature roasting furnace can be absorbed by water to obtain ammonia water.
[0041] Specifically, a gas collecting device is connected to the high temperature roasting furnace, that is, the gas collecting device is connected to the exhaust end of the high temperature roasting furnace. The gas collected from the exhaust end of the high temperature roasting furnace is absorbed by water, where the water can be industrial pure water, and the water is used to collect the ammonia generated in the roasting reaction. The absorption method may include a spray method and a bubbling method, and the product obtained after collection is ammonia water. For example, a spray tower can be used.
[0042] Second Exemplary Embodiment
[0043] In a second exemplary embodiment of the present invention, a magnesium sulfate solution and ammonia water are provided, wherein the magnesium sulfate solution and ammonia water are obtained by the above-mentioned method for refining magnesium sulfate solution from asbestos tailings.
[0044] Third Exemplary Embodiment
[0045] In a third exemplary embodiment of the present invention, a method for applying a magnesium sulfate solution is provided, the method comprising the following steps:
[0046] A1. Use the refined magnesium sulfate solution described above.
[0047] A2, directly evaporating and crystallizing the refined magnesium sulfate solution to obtain refined magnesium sulfate; or adding ammonia water to the refined magnesium sulfate solution to neutralize and precipitate, filtering, and drying the filter residue to obtain magnesium hydroxide powder; or adding ammonia water to the refined magnesium sulfate solution, passing CO2 to neutralize and heat to precipitate, filtering, and drying the filter residue to obtain basic magnesium carbonate powder, the filtered filtrate is ammonium sulfate solution, and the ammonium sulfate solution is evaporated and crystallized to obtain ammonium sulfate powder.
[0048] In order to better understand the above exemplary embodiments of the present invention, a refined magnesium sulfate solution from asbestos tailings and a method and application thereof are described below in conjunction with specific examples.
[0049] Example 1
[0050] The mineral types contained in the Aksai asbestos tailings selected for the test are mainly serpentine, with a small amount of talc, magnetite and quartz. The main chemical compositions are shown in Table 1:
[0051] Table 1 Main chemical components of asbestos tailings
[0052] element <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[TFe2O3]]> MgO CaO Loss on ignition other <![CDATA[Content w B / %]]> 40.33 1.20 3.09 41.59 0.47 12.74 0.58
[0053] The method for refining magnesium sulfate solution from asbestos tailings comprises the following steps:
[0054] (1) Ammonium sulfate and asbestos tailing powder were mixed in a molar ratio of 0.75 and placed in a high-temperature furnace for calcination at 650° C. for 120 min to obtain a calcined activated product. The calcined activated product mainly contained magnesium sulfate, magnesium sulfate hexahydrate, hematite, forsterite, unreacted serpentine and a small amount of quartz.
[0055] (2) A spray tower filled with industrial pure water is connected to the end of the high-temperature roasting furnace to collect ammonia gas and obtain ammonia water.
[0056] (3) The calcined activated asbestos tailings were placed in a reactor with stirring and heating functions, a dilute sulfuric acid solution with a pH value of 6 was added to the reactor, and the reaction was carried out for 60 minutes at a temperature of 25° C. and a liquid-solid ratio of 20 ml / g, and the product after the reaction was filtered to obtain a refined magnesium sulfate solution. The concentration of iron ions in the filtrate was 0.69 mg / L, and the concentration of magnesium ions was 5.83 g / L; the leaching rate of iron ions in the asbestos tailings was 0.05%, and the leaching rate of magnesium ions was 77.09%.
[0057] (4) Refined magnesium sulfate is obtained by direct evaporation and crystallization of the refined magnesium sulfate solution. The iron ion content of the magnesium sulfate is less than 0.0005, which meets the high-grade purity standard in "Chemical Reagent Magnesium Sulfate" (GB / T 671-1998).
[0058] Figure 2The XRD diagrams of the roasting reaction product and the leaching residue of Example 1 of the present invention are shown. It can be seen that the main phase compositions of the roasting residue are magnesium sulfate, magnesium sulfate hexahydrate, hematite, unreacted serpentine, forsterite and quartz, and the main phase compositions of the leaching residue are hematite, unreacted serpentine, forsterite and quartz. Figure 2 The upper line segment is the leached residue, and the lower line segment is the roasted residue. Since the content of forsterite and quartz in the roasted residue is low, it is difficult to see in the XRD spectrum, but through the analysis of the water leached residue XRD, it can be seen that forsterite and quartz are present in the water leached residue, so it is obtained that the roasted residue contains forsterite and quartz.
[0059] Example 2
[0060] The mineral types contained in the Qinghai Mangya asbestos tailings selected for the test are mainly serpentine, with a small amount of talc, magnetite and quartz. The main chemical compositions are shown in Table 2:
[0061] Table 2 Main chemical components of asbestos tailings
[0062] element <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[TFe2O3]]> MgO CaO Loss on ignition other <![CDATA[Content w B / %]]> 37.89 0.81 6.91 40.25 0.54 13.03 0.57
[0063] (1) Ammonium bisulfate and asbestos tailing powder were mixed in a molar ratio of 1.5 and placed in a high-temperature furnace for roasting at 750° C. for 60 min to obtain a roasted activated product. The roasted activated product mainly contained minerals such as magnesium sulfate, magnesium sulfate hexahydrate, hematite, forsterite and a small amount of quartz.
[0064] (2) A spray tower filled with industrial pure water is connected to the end of the high-temperature roasting furnace to collect ammonia gas and obtain ammonia water.
[0065] (3) The asbestos tailings after roasting and activation are placed in a reactor with stirring and heating functions, and dilute sulfuric acid with a pH value of 5 is added to the reactor. The reaction is carried out at a temperature of 50°C and a liquid-solid ratio of 20ml / g for 30 minutes. The product after the reaction is filtered to obtain a refined magnesium sulfate solution. The concentration of iron ions in the filtrate is 0.32mg / L, and the concentration of magnesium ions is 7.35g / L; the leaching rate of iron ions in the asbestos tailings is 0.80%, and the leaching rate of magnesium ions is 97.19%. (4) The refined magnesium sulfate solution is directly evaporated and crystallized to obtain refined magnesium sulfate, and the iron ion content in the magnesium sulfate is less than 0.0005, which meets the high-grade purity standard in "Chemical Reagent Magnesium Sulfate" (GB / T671-1998).
[0066] Example 3
[0067] The mineral types contained in the Aksai asbestos tailings selected for the test are mainly serpentine, with a small amount of talc, magnetite and quartz. The main chemical compositions are shown in Table 3:
[0068] Table 3 Main chemical components of asbestos tailings
[0069] element <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[TFe2O3]]> MgO CaO Loss on ignition other <![CDATA[Content w B / %]]> 40.33 1.20 3.09 41.59 0.47 12.74 0.58
[0070] (1) Ammonium sulfate and asbestos tailing powder were mixed in a molar ratio of 1.0 and placed in a high-temperature furnace, and calcined at 650° C. for 60 min to obtain a calcined activated product. The calcined activated product mainly contained minerals such as magnesium sulfate, magnesium sulfate hexahydrate, hematite, forsterite, unreacted serpentine and a small amount of quartz.
[0071] (2) A reaction tank filled with industrial pure water is connected to the end of the high-temperature roasting furnace to collect ammonia gas by bubbling to obtain ammonia water.
[0072] (3) The calcined activated asbestos tailings were placed in a reactor with stirring and heating functions, and dilute sulfuric acid with a pH value of 6.8 was added to the reactor. The reaction was carried out at a temperature of 25° C. and a liquid-solid ratio of 8 ml / g for 60 minutes. The product after the reaction was filtered to obtain a refined magnesium sulfate solution. The concentration of iron ions in the filtrate was 2.3 mg / L, and the concentration of magnesium ions was 12.24 g / L; the leaching rate of iron ions in the asbestos tailings was 0.08%, and the leaching rate of magnesium ions was 84.18%.
[0073] (4) Refined magnesium sulfate is obtained by direct evaporation and crystallization of the refined magnesium sulfate solution. The iron ion content of the magnesium sulfate is less than 0.0005, which meets the high-grade purity standard in "Chemical Reagent Magnesium Sulfate" (GB / T 671-1998).
[0074] Example 4
[0075] The mineral types contained in the Shaanxi Da'an asbestos tailings selected for the test are mainly serpentine, with a small amount of talc, magnetite, chlorite, brucite and quartz. The main chemical compositions are shown in Table 4:
[0076] Table 4 Main chemical components of asbestos tailings
[0077] element <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[TFe2O3]]> MgO CaO Loss on ignition other <![CDATA[Content w B / %]]> 37.69 1.20 7.75 40.13 0.42 12.5 0.31
[0078] (1) Ammonium sulfate and asbestos tailing powder were mixed in a molar ratio of 1.0 and placed in a high-temperature furnace for roasting at 650° C. for 60 min to obtain a roasted activated product. The roasted activated product mainly contained magnesium sulfate, magnesium sulfate hexahydrate, hematite, forsterite and a small amount of quartz.
[0079] (2) A reaction tank filled with industrial pure water is connected to the end of the high-temperature roasting furnace to collect ammonia gas by bubbling to obtain ammonia water.
[0080] (3) The calcined activated asbestos tailings were placed in a reactor with stirring and heating functions, and dilute sulfuric acid with a pH value of 6 was added to the reactor. The reaction was carried out at a temperature of 40° C. and a liquid-solid ratio of 16 ml / g for 90 minutes. The product after the reaction was filtered to obtain a refined magnesium sulfate solution. The concentration of iron ions in the filtrate was 0.46 mg / L, and the concentration of magnesium ions was 7.79 g / L; the leaching rate of iron ions in the asbestos tailings was 0.03%, and the leaching rate of magnesium ions was 86.45%.
[0081] (4) Refined magnesium sulfate is obtained by direct evaporation and crystallization of the refined magnesium sulfate solution. The iron ion content of the magnesium sulfate is less than 0.0005, which meets the high-grade purity standard in "Chemical Reagent Magnesium Sulfate" (GB / T 671-1998).
[0082] Example 5
[0083] The mineral types contained in the Qinghai Mangya asbestos tailings selected for the test are mainly serpentine, with a small amount of talc, magnetite and brucite. The main chemical compositions are shown in Table 5:
[0084] Table 5 Main chemical components of asbestos tailings
[0085] element <![CDATA[SiO2]]> <![CDATA[Al2O3]]> <![CDATA[TFe2O3]]> MgO CaO Loss on ignition other <![CDATA[Content w B / %]]> 37.89 0.81 6.91 40.25 0.54 13.03 0.57
[0086] (1) Ammonium sulfate and asbestos tailing powder were mixed in a molar ratio of 1.25 and placed in a high-temperature furnace for roasting at 650° C. for 90 min to obtain a roasted activated product. The roasted activated product mainly contained magnesium sulfate, magnesium sulfate hexahydrate, hematite, forsterite, unreacted serpentine and a small amount of quartz.
[0087] (2) A spray tower filled with industrial pure water is connected to the end of the high-temperature roasting furnace to collect ammonia gas and obtain ammonia water.
[0088] (3) The asbestos tailings after calcination and activation were placed in a reactor with stirring and heating functions, and dilute sulfuric acid with a pH value of 5 was added to the reactor. The reaction was carried out at a temperature of 25° C. and a liquid-solid ratio of 12 ml / g for 60 minutes. The product after the reaction was filtered to obtain a refined magnesium sulfate solution. The concentration of iron ions in the filtrate was 0.92 mg / L, and the concentration of magnesium ions was 9.38 g / L; the leaching rate of iron ions in the asbestos tailings was 0.04%, and the leaching rate of magnesium ions was 84.31%.
[0089] (4) Refined magnesium sulfate is obtained by direct evaporation and crystallization of the refined magnesium sulfate solution. The iron ion content of the magnesium sulfate is less than 0.0005, which meets the high-grade purity standard in "Chemical Reagent Magnesium Sulfate" (GB / T 671-1998).
[0090] In summary, the green processing method of the present invention for directly obtaining a refined magnesium sulfate solution by roasting-leaching can not only make resource utilization of asbestos tailings, save land resources, and protect the environment, but also is easy to operate. By roasting with an auxiliary agent, iron ions are converted into hematite and retained in the filter residue, and a refined magnesium sulfate solution with an extremely low iron ion concentration is obtained. The leaching rate of magnesium ions is stabilized at more than 77%, and the leaching rate of iron ions is stabilized at less than 0.8%.
[0091] Although the present invention has been described above by combining with exemplary embodiments, it will be apparent to those skilled in the art that various modifications and changes may be made to the exemplary embodiments of the present invention without departing from the spirit and scope defined in the claims.
Claims
1. A method for refining magnesium sulfate solution from asbestos tailings, It is characterized in that The method for refining magnesium sulfate solution from asbestos tailings comprises the following steps: The asbestos tailing powder and the reaction aid are mixed evenly, and placed in a high-temperature roasting furnace for roasting treatment to obtain a roasting reaction product and a gas collected at the exhaust end of the high-temperature roasting furnace; the roasting treatment temperature is 650-750° C., and the roasting treatment time is 60-120 minutes; The roasting reaction product is leached and filtered in a reaction kettle, and the filtrate is a refined magnesium sulfate solution; The concentration of Mg ions in the refined magnesium sulfate solution is 5.67-12.25 g / L, and the concentration of Fe ions is 0.32-2.30 mg / L; The leaching step comprises: adding a dilute sulfuric acid solution with a pH value of 5 to 6.8 to the roasting reaction product in a reaction kettle, reacting for 30 to 90 minutes at 25 to 50° C. and a liquid-to-solid ratio of 8 to 20 ml / g; Wherein, the reaction aid comprises ammonium sulfate powder and / or ammonium hydrogen sulfate powder; the molar ratio of the reaction aid to the asbestos tailing powder is 0.75-1.50:1; The asbestos tailings are calculated by mass percentage, and the amount of each component is 37.0% to 42.0% SiO 2 , 36.0% to 42.0% MgO, 0.8% to 1.2% Al 2 O 3 , 3.0%~8.0% TFe 2 O 3 and 0.4% to 0.7% CaO, the loss on ignition is 12.0% to 13.5%; The mineral types of the roasting reaction product are mainly magnesium sulfate and magnesium sulfate hexahydrate, and also include hematite, forsterite, unreacted serpentine and quartz; The leaching rate of Mg ions in the asbestos tailings powder is 77-97%, and the leaching rate of Fe ions is 0.03-0.80%.
2. The method for refining magnesium sulfate solution from asbestos tailings according to claim 1, It is characterized in that The method for refining magnesium sulfate solution from asbestos tailings also includes: The gas collected from the exhaust end of the high-temperature roasting furnace is absorbed by water to obtain ammonia water.
3. The method for refining magnesium sulfate solution from asbestos tailings according to claim 1, It is characterized in that The preparation of the ammonium sulfate powder comprises the following steps: Add ammonia water to the refined magnesium sulfate solution and pass CO 2 The product is neutralized, heated and precipitated, filtered and the filter residue is dried to obtain basic magnesium carbonate powder. The filtered filtrate is an ammonium sulfate solution. The ammonium sulfate solution is evaporated and crystallized to obtain ammonium sulfate powder.
4. The method for refining magnesium sulfate solution from asbestos tailings according to claim 2, It is characterized in that The absorption includes a spraying method and / or a bubbling method.
5. A magnesium sulfate solution, It is characterized in that The magnesium sulfate solution is obtained by the method for refining magnesium sulfate solution from asbestos tailings according to any one of claims 1 to 4.
6. Application of a magnesium sulfate solution, It is characterized in that The application method comprises the following steps: Using the refined magnesium sulfate solution according to claim 5; Directly evaporating and crystallizing the refined magnesium sulfate solution to obtain refined magnesium sulfate; or Adding ammonia water to the refined magnesium sulfate solution for neutralization and precipitation, filtering, and drying the filter residue to obtain magnesium hydroxide powder; or Add ammonia water to the refined magnesium sulfate solution and pass CO 2 The product is neutralized, heated and precipitated, filtered and the filter residue is dried to obtain basic magnesium carbonate powder. The filtered filtrate is an ammonium sulfate solution. The ammonium sulfate solution is evaporated and crystallized to obtain ammonium sulfate powder.