A heterogeneous catalyst and its preparation method and application in olefin polymerization
Through the method of supporting catalyst, the spatial distribution of catalytic components in the particles is adjusted, and the problems of insufficient alloy material performance in the polyolefin kettle and the scaling of the reactor are solved, thereby achieving the preparation of high-performance polymers and energy savings.
Patent Information
- Application Number
- CN202310135327.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-02-09
Smart Images

Figure CN116082543B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalytic olefin polymerization, and in particular to a multiphase catalyst and a preparation method thereof and application thereof in olefin polymerization reactions. Background Art
[0002] Polyethylene autoclave alloy refers to a polyethylene alloy obtained directly from the reaction monomer ethylene by autoclave polymerization, thereby replacing the traditional blending method of melt blending polymers. The development of polyolefin autoclave alloy technology has always been accompanied by the continuous improvement and development of Ziegler-natta catalyst technology and metallocene catalyst technology. For a long time, catalytic research has mainly focused on improving the activity of catalysts and controlling the molecular structure of polyolefins. In recent years, polyolefin autoclave alloys prepared using dual-active center catalysts and reactor blending technology have received a lot of attention. Because the blend in the reactor can combine the performance advantages of different components, high-performance polyolefin materials for different uses can be prepared.
[0003] Since the development of Ziegler-Natta in the 1950s, the engineering methods for the preparation of polyolefin in-reactor alloys have mainly been reactor cascades and multi-zone reactor technologies. Since the 1980s, the application of dual-site catalysts composed of different single-site molecular catalysts in the synthesis of polyolefin in-reactor alloys has received increasing attention. For homogeneous catalysts, the control of polymer morphology cannot be achieved when used alone, which brings about the technical problem of reactor fouling. The existence of this problem is not conducive to the stable operation of the polymerization reaction unit and leads to a significant increase in the cleaning cost of the reactor. In contrast, dual-site molecular catalysts can better control the polymerization reaction and produce a wide range of polyolefins for different applications. In industry, since heterogeneous dual-site catalysts can be controlled in product morphology, they are preferred for use in industrial production. The use of heterogeneous catalysts avoids the typical reactor fouling in slurry polymerization and gas phase polymerization of homogeneous systems. Compared with melt blending, the above-mentioned in-reactor blending process can mix different polyolefins in the mesoscopic range without the need for high temperatures and extensive shearing. Therefore, considerable cost and energy savings are provided, and more efficient dispersion is achieved.
[0004] The Chinese patent application document with publication number CN110026196A discloses a supported heterogeneous catalyst and its preparation method and application. The supported heterogeneous catalyst provided by the patent includes aluminum oxide nanotubes and cobalt oxide deposited on the outer surface of the aluminum oxide nanotubes. The patent uses aluminum oxide nanotubes as carriers and deposits cobalt oxide as an active component on the outer surface of the carrier, which can make the active component evenly dispersed, thereby obtaining a catalyst with higher activity. The results of the examples show that when the catalyst provided by the patent is used for the epoxidation reaction of styrene, the selectivity reaches 74.3-94.8%, and the conversion rate reaches 77.2-91.4%. However, the patent does not involve the preparation of alloy materials in olefin kettles, nor does it involve the mesoscopic control of the ultrastructure of alloys in olefin kettles, so it needs further improvement. Summary of the invention
[0005] The technical problem to be solved by the present invention is how to prepare a multiphase catalyst to achieve radial distribution regulation at the nanoscale, so as to be used for preparing polyolefin kettle alloy material and further improve the performance of the material.
[0006] The present invention solves the above technical problems through the following technical means:
[0007] The first aspect of the present invention provides a method for preparing a heterogeneous catalyst, comprising the following steps:
[0008] S1: adding a metal salt type polar monomer and an organic solvent to a reaction container at room temperature under magnetic stirring to dissolve them, adding a co-catalyst, and then adding an α-diimine nickel catalyst or a mixed solution of two different α-diimine nickel catalysts;
[0009] S2: After stirring and mixing evenly, let it stand for reaction to obtain;
[0010] or
[0011] P1: Add an α-diimine nickel catalyst, a metal salt type polar monomer and an organic solvent into a reaction vessel at room temperature under magnetic stirring to dissolve them;
[0012] P2: Add a co-catalyst, and then add another α-diimine nickel catalyst, stir and mix evenly, and let it stand to react to obtain;
[0013] or
[0014] Q1: At room temperature, under magnetic stirring, add an α-diimine nickel catalyst, a metal salt type polar monomer and an organic solvent into a reaction container to dissolve them, add a co-catalyst, and stir to mix evenly;
[0015] Q2: Add another α-diimine nickel catalyst and a metal salt type polar monomer, then add an organic solvent to dissolve them, then add a co-catalyst, stir and mix evenly, and let stand to react to obtain;
[0016] The metal salt type polar monomers are all di(10-undecenoic acid)aluminum chloride.
[0017] Beneficial effects: The present invention utilizes the supported catalyst to prepare a multiphase catalyst, solves the coordination precipitation polymerization of monomers, adjusts the spatial distribution of different catalytic components in the particles, and realizes controllable catalyst morphology. The catalyst is used to prepare polyolefin kettle alloy materials, which improves the performance of the product. The obtained polyolefin kettle alloy has excellent mechanical and rheological properties.
[0018] Preferably, the α-diimine nickel catalysts all have the structural formula:
[0019] catalyst.
[0020] Preferably, the organic solvents are one or more of petroleum ether, pentane, hexane, heptane, octane, hydrogenated gasoline, isoparaffins, methylcyclohexane, decalin, methylcyclohexane, cyclohexane, benzene, toluene, xylene, saturated isoparaffins, hydrogenated gasoline, dichloromethane, chloroform, chlorobenzene and dichlorobenzene.
[0021] Preferably, the co-catalyst is one or more of diethylaluminum chloride, methylaluminoxane, ethylaluminum dichloride, triisobutylaluminum and tris(pentafluorophenyl)boron.
[0022] Preferably, the molar ratio of the two different α-diimine nickel catalysts in step S1 is 1:4 to 4:1.
[0023] Preferably, the molar ratio of the two different α-diimine nickel catalysts in step S1 is 1:4, 1:2, 1:1, 2:1 or 4:1.
[0024] Preferably, the molar ratio of one α-diimine nickel catalyst in step P1 to another α-diimine nickel catalyst in step P2 is 1:4 to 4:1.
[0025] Preferably, the molar ratio of one α-diimine nickel catalyst in step P1 to another α-diimine nickel catalyst in step P2 is 1:4, 1:2, 1:1, 2:1 or 4:1.
[0026] Preferably, the molar ratio of one α-diimine nickel catalyst in step Q1 to another α-diimine nickel catalyst in step Q2 is 1:4 to 4:1.
[0027] Preferably, the molar ratio of one α-diimine nickel catalyst in step Q1 to another α-diimine nickel catalyst in step Q2 is 1:4, 1:2, 1:1, 2:1 or 4:1.
[0028] Preferably, the temperature of the static reaction is 5 to 25°C.
[0029] Preferably, the static reaction time is 4 to 8 hours.
[0030] The second aspect of the present invention provides a heterogeneous catalyst prepared using the above method.
[0031] The third aspect of the present invention provides an application of the multiphase catalyst prepared by the above method in olefin polymerization reaction.
[0032] The advantages of the present invention are:
[0033] 1. The present invention utilizes the supported catalyst to prepare a multiphase catalyst, solves the coordination precipitation polymerization of monomers, adjusts the spatial distribution of different catalytic components in the particles, and realizes controllable catalyst morphology. The catalyst is used to prepare polyolefin kettle alloy materials, which improves the performance of the product. The obtained polyolefin kettle alloy has excellent mechanical and rheological properties.
[0034] 2. The present invention adopts a self-supporting strategy based on Brookhart-type nickel-catalyzed precipitation polymerization of polar monomer metal salt of 10-undecenoic acid (UA-Al), which not only realizes the self-supporting isomerization of nickel catalyst, but also adjusts the spatial distribution of different catalytic components in the particles. The obtained heterogeneous multi-center catalyst is used for chain-step polymerization of ethylene to generate an in-vessel alloy composed of polyethylene with different branching densities.
[0035] 3. Since the polyolefin in-reactor alloy is prepared by a multi-phase dual-site catalyst, the scaling in the reactor during the reaction can be reduced. In addition, high temperature and extensive shearing are not required, which saves energy.
[0036] 4. The polyolefin in-reactor alloy material obtained by the present invention has excellent adjustable performance. The microstructural regulation achieved by the dual-position catalyst can not only solve the coordination precipitation polymerization problem of polar monomers, but also achieve the morphology regulation of polymers.
[0037] 5. The poly(ethylene-olefin acid aluminum salt) copolymer alloy material obtained by the present invention contains a polar polyolefin acid aluminum salt component, thereby improving the compatibility with polylactic acid materials. The prepared poly(ethylene-olefin acid aluminum salt)-polylactic acid blend alloy material has better mechanical properties than the poly(ethylene-olefin acid aluminum salt) binary copolymer alloy material.
[0038] 6. The multiphase dual catalyst of the present invention is used to control the radial distribution of the nanoscale for preparing polyolefin in-reactor alloys. The co-loading of the dual catalysts is achieved by the coordination precipitation homopolymerization of the dual catalysts and polar monomer metal salts. The obtained dual-site catalyst can prepare powdered polymers in ethylene homopolymerization or copolymerization reactions, avoiding scaling in the reactor. In addition, the obtained polyolefin in-reactor alloy has excellent mechanical and rheological properties, and its material properties can be adjusted by the radial distribution of the dual-site catalyst at the nanoscale. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Schematic diagram of the co-precipitation self-support of Brookhart-type nickel catalyst during polymerization and the precipitation polymerization of UA-Al;
[0040] Figure 2 A schematic diagram of the morphology and structure of the multiphase catalyst prepared in Example 3-11 of the present invention;
[0041] Figure 3 This is a scanning electron microscope image of the heterogeneous catalyst A@UA-Al homopolymer prepared in Example 1 of the present invention;
[0042] Figure 4 This is a scanning electron microscope image of the heterogeneous catalyst B@UA-Al homopolymer prepared in Example 2 of the present invention;
[0043] Figure 5 This is a scanning electron microscope image of the heterogeneous catalyst AB(1 / 1)@UA-Al homopolymer prepared in Example 3 of the present invention;
[0044] Figure 6 This is a scanning electron microscope image of the heterogeneous catalyst A / B (1 / 1) @ UA-Al homopolymer prepared in Example 5 of the present invention;
[0045] Figure 7 This is a scanning electron microscope image of the heterogeneous catalyst B / A(1 / 1)@UA-Al homopolymer prepared in Example 6 of the present invention;
[0046] Figure 8 A comparison chart of the tensile strength of the alloy materials in the polyethylene kettle prepared in Application Examples 1-7, Application Example 9 and Comparative Example 3 of the present invention;
[0047] Fig. 9 It is a comparison chart of the elongation at break of the alloy materials in the polyethylene kettle prepared in Application Examples 1-7, Application Example 9 and Comparative Example 3 of the present invention;
[0048] Fig.10 This is a comparison chart of the toughness of the alloy materials in the polyethylene kettle obtained in Application Examples 1-7, Application Example 9 and Comparative Example 3 of the present invention;
[0049] Fig.11A comparison chart of Young's modulus of alloy materials in polyethylene kettles prepared in Application Examples 1-7, Application Example 9 and Comparative Example 3 of the present invention;
[0050] Fig.12 The DSC curve diagram of the alloy material in the polyethylene kettle obtained in Application Examples 3-6 of the present invention;
[0051] Fig.13 It is a comparison chart of the melt stock modulus of the blends in the polyethylene reactor of Application Examples 3-6 of the present invention and Comparative Example 3;
[0052] Fig.14 Based on Fig.13 Comparison of the obtained modulus improvement rates;
[0053] Fig.15 Schematic diagram of the structure of AB-type heterogeneous dual-site catalyst at the microscopic scale;
[0054] Fig.16 It is a strain-stress comparison diagram of Application Example 12 and Comparative Examples 4-5. DETAILED DESCRIPTION
[0055] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0056] In the method of the present invention, the α-diimine nickel metal catalyst used as a starting material may be any α-diimine nickel metal catalyst known in the art, which may be commercially available or conveniently prepared by methods known in the art.
[0057] Embodiment 1:
[0058] For the convenience of description, the structural formula is:
[0059] The α-diimine nickel catalyst, named NiA, was prepared according to the method in the literature (Polymer 2017, 127, 88-100).
[0060] The structural formula is:
[0061] The α-diimine nickel catalyst is named NiB, and the NiB catalyst is also prepared according to the method reported in the literature (Polymer 2017, 127, 88-100).
[0062] The α-diimine nickel (A) heterogeneous single-site catalyst supported on di(10-undecenoic acid)aluminum monochloride is named A@UA-Al for the convenience of description.
[0063] The preparation method of the heterogeneous catalyst A@UA-Al comprises the following steps:
[0064] (1) At room temperature, under magnetic stirring at 1000 r / min, add 10 mL of n-heptane and 1.5 mmol of di(10-undecenoic acid)aluminum chloride into a thick-walled glass pressure vessel to dissolve them;
[0065] (2) Add 1 mmol of diethylaluminum chloride, and then add 2 μmol of NiA, wherein NiA is dissolved in 0.2 mL of dichloromethane. After stirring and mixing, the system is cooled to 5°C and allowed to react for 8 hours. The resulting reaction mixture dispersion is then cooled to -20°C and stored.
[0066] Embodiment 2:
[0067] The α-diimine nickel (B) heterogeneous single-site catalyst supported on di(10-undecenoic acid)aluminum monochloride is named as B@UA-Al for the convenience of description.
[0068] The preparation method of the multiphase catalyst B@UA-Al is different from that of Example 1 in that "NiA" is changed to "NiB" and the other steps are the same as those of Example 1.
[0069] Embodiment 3:
[0070] The α-diimine nickel (AB) heterogeneous dual-site catalyst supported by di(10-undecenoic acid) aluminum chloride, in which the molar ratio of NiA to NiB is 1:1, is named: AB(1 / 1)@UA-Al for the convenience of description.
[0071] The preparation method of the multiphase dual-position catalyst AB (1 / 1) @ UA-Al comprises the following steps:
[0072] (1) At room temperature, 0.65 μmol NiA catalyst and 0.65 μmol NiB catalyst were mixed in 0.13 mL dichloromethane to obtain a mixed solution containing catalysts NiA and NiB;
[0073] (2) under magnetic stirring at 1500 r / min, 1 mmol of di(10-undecenoic acid)aluminum chloride was added to a 20 mL glass reaction bottle, and then 10 mL of heptane was added to dissolve it, 0.65 mmol of diethylaluminum chloride was added, and then the mixed solution obtained in step (1) was added;
[0074] (3) After stirring and mixing, the mixture was allowed to react at 25°C for 4 h, and then the obtained reaction mixture dispersion was cooled to -20°C for storage.
[0075] Embodiment 4:
[0076] The α-diimine nickel (A+B) heterogeneous dual-site catalyst supported on di(10-undecenoic acid) aluminum chloride, in which the molar ratio of NiA to NiB is 1:1, is named A+B(1 / 1)@UA-Al for the convenience of description.
[0077] The multi-phase dual catalyst The preparation method of A+B(1 / 1)@UA-Al comprises the following steps:
[0078] (1) At room temperature, under magnetic stirring at 1500 r / min, 0.65 μmol NiA catalyst, 1 mmol di(10-undecenoic acid)aluminum chloride and 10 mL heptane were added into a 20 mL glass reaction bottle to dissolve them;
[0079] (2) 0.65 mmol of diethylaluminum chloride was added, followed by 0.65 μmol of NiB catalyst, and the mixture was stirred and mixed uniformly. The mixture was allowed to react at 20° C. for 6 h, and the obtained reaction mixture dispersion was then cooled to −20° C. for storage.
[0080] Embodiment 5:
[0081] The α-diimine nickel (A / B) heterogeneous dual-site catalyst supported on di(10-undecenoic acid) aluminum chloride, in which the molar ratio of NiA to NiB is 1:1, is named A / B(1 / 1)@UA-Al for the convenience of description.
[0082] The preparation method of the multiphase dual-position catalyst A / B (1 / 1) @ UA-Al comprises the following steps:
[0083] (1) At room temperature, under magnetic stirring at 1500 r / min, 0.65 μmol NiB catalyst, 0.5 mmol di(10-undecenoic acid)aluminum chloride and 5 mL heptane were added to a 20 mL glass reaction bottle to dissolve them, and 0.33 mmol diethylaluminum chloride was added and stirred to mix well;
[0084] (2) 0.65 μmol NiA catalyst and 0.5 mmol di(10-undecenoic acid)aluminum chloride were added, and then 5 mL of heptane was added to dissolve them. Then 0.32 mmol of diethylaluminum chloride was added, and after stirring and mixing evenly, the mixture was allowed to stand at 25°C for 4 h. Then, the obtained reaction mixture dispersion was cooled to -20°C for storage.
[0085] A / B and B / A core-shell catalysts were prepared using a two-step nickel-catalyzed precipitation polymerization method. In the second step, a layer of polymer-supported B or A catalyst was deposited on the surface of the prefabricated A or B heterogeneous unit catalyst to obtain a core-shell superstructure (A / B (1 / 1), B / A (1 / 1)).
[0086] The obtained catalyst particles were characterized using scanning electron microscopy. The scanning electron microscopy images showed that the heterogeneous catalyst particles obtained by two-step precipitation polymerization were significantly larger than the catalyst particles obtained by one-step precipitation polymerization, indicating that the formation of the core-shell superstructure is based on secondary deposition.
[0087] Embodiment 6:
[0088] The α-diimine nickel (B / A) heterogeneous dual-site catalyst supported on di(10-undecenoic acid) aluminum chloride, in which the molar ratio of NiA to NiB is 1:1, is named B / A(1 / 1)@UA-Al for the convenience of description.
[0089] The preparation method of the multiphase dual-position catalyst B / A(1 / 1)@UA-Al comprises the following steps:
[0090] (1) At room temperature, under magnetic stirring at 1500 r / min, 0.65 μmol NiA catalyst, 0.5 mmol di(10-undecenoic acid)aluminum chloride and 5 mL heptane were added to a 20 mL glass reaction bottle to dissolve them, and 0.33 mmol diethylaluminum chloride was added and stirred to mix well;
[0091] (2) Then, 0.65 μmol NiB catalyst and 0.5 mmol di(10-undecenoic acid)aluminum chloride were added, and then 5 mL of heptane was added to dissolve them. Then, 0.32 mmol of diethylaluminum chloride was added, and after stirring and mixing evenly, the mixture was allowed to stand at 25° C. for a period of time, and then the obtained reaction mixture dispersion was cooled to -20° C. for storage.
[0092] Embodiment 7:
[0093] The α-diimine nickel (AB) heterogeneous dual-site catalyst supported by di(10-undecenoic acid) aluminum chloride, in which the molar ratio of NiA to NiB is 1:2, is named: AB(1 / 2)@UA-Al for the convenience of description.
[0094] The preparation method of the multiphase dual-site catalyst AB(1 / 2)@UA-Al is different from that of Example 3 in that "0.65 μmol NiB" is changed to "1.30 μmol NiB", and the other steps are the same as those of Example 3.
[0095] Embodiment 8:
[0096] The α-diimine nickel (AB) heterogeneous dual-site catalyst supported by di(10-undecenoic acid) aluminum chloride, in which the molar ratio of NiA to NiB is 1:4, is named: AB(1 / 4)@UA-Al for the convenience of description.
[0097] The preparation method of the multiphase dual-site catalyst AB(1 / 4)@UA-Al is different from that of Example 3 in that "0.65 μmol NiB" is changed to "2.60 μmol NiB", and the other steps are the same as those of Example 3.
[0098] Embodiment 9:
[0099] The α-diimine nickel (AB) heterogeneous dual-site catalyst supported by di(10-undecenoic acid) aluminum chloride, in which the molar ratio of NiA to NiB is 2:1, is named: AB(2 / 1)@UA-Al for the convenience of description.
[0100] The preparation method of the multiphase dual-site catalyst AB (2 / 1) @ UA-Al is different from that of Example 3 in that "0.65 μmol NiA" is changed to "1.30 μmol NiA", and the other steps are the same as those of Example 3.
[0101] Embodiment 10:
[0102] The α-diimine nickel (AB) heterogeneous dual-site catalyst supported by di(10-undecenoic acid) aluminum chloride, in which the molar ratio of NiA to NiB is 4:1, is named: AB(4 / 1)@UA-Al for the convenience of description.
[0103] The preparation method of the multiphase dual-site catalyst AB (4 / 1) @ UA-Al is different from that of Example 3 in that "0.65 μmol NiA" is changed to "2.60 μmol NiA", and the other steps are the same as those of Example 3.
[0104] Embodiment 11:
[0105] The α-diimine nickel (A / B) heterogeneous dual-site catalyst supported on di(10-undecenoic acid) aluminum chloride, in which the molar ratio of NiA to NiB is 4:1, is named A / B(4 / 1)@UA-Al for the convenience of description.
[0106] The preparation method of the multiphase dual-position catalyst A / B (4 / 1) @ UA-Al is different from that of Example 5 in that "0.65 μmol NiA" is changed to "2.60 μmol NiA", and the other steps are the same as those of Example 5.
[0107] Application Example 1: Ethylene Homopolymerization Using Heterogeneous Catalysts
[0108] The alloy material in the polyethylene reactor was prepared using the heterogeneous catalyst prepared in Example 1. Specifically, in a 350 ml glass thick-walled pressure vessel, 70 ml of n-heptane and 1.3 μmol of the heterogeneous catalyst prepared in Example 1 were placed in a glove box, the pressure vessel was connected to a high-pressure pipeline, and then the solution was degassed; the vessel was cooled to 5° C. and allowed to react for 10 minutes. Under rapid stirring, the reactor was pressurized with 0.8 MPa of ethylene. After 30 minutes, the pressure vessel was vented, and the polymer was precipitated in acidified ethanol (ethanol / 37% HCl=50 / 1), and dried in a vacuum at 50° C. for 24 hours. The results are summarized in Table 1 below.
[0109] Application Example 2-11: Ethylene Homopolymerization Using Heterogeneous Catalysts
[0110] The difference between Application Examples 2-11 and Application Example 1 is that "the heterogeneous catalyst prepared in Examples 2-11" is used to replace "the heterogeneous catalyst prepared in Example 1", and the other steps are the same as those in Application Example 1. The results are summarized in Table 1 below.
[0111] Comparative Example 1: Use of NiA homogeneous catalyst for ethylene polymerization
[0112] The difference between this comparative example and application example 1 is that "NiA homogeneous catalyst" is used to replace "the heterogeneous catalyst prepared in Example 1" and the other steps are the same as those in application example 1. The results are summarized in Table 1 below.
[0113] Comparative Example 2: Use of NiB homogeneous catalyst for ethylene polymerization
[0114] The difference between this comparative example and application example 1 is that "NiB homogeneous catalyst" is used to replace "the heterogeneous catalyst prepared in Example 1" and the other steps are the same as those in application example 1. The results are summarized in Table 1 below.
[0115] Comparative Example 3: Use of NiAB (1 / 1) homogeneous catalyst for ethylene polymerization
[0116] The difference between this comparative example and application example 1 is that "NiA and NiB homogeneous catalyst with a molar ratio of 1:1" is used to replace the "heterogeneous catalyst prepared in Example 1" and the other steps are the same as those in application example 1. The results are summarized in Table 1 below.
[0117] Table 1: Ethylene polymerization catalyzed by homogeneous and heterogeneous catalysts
[0118]
[0119]
[0120] aPolymerization conditions: catalyst dosage 1.3 μmol, n-heptane 70 mL, ethylene pressure 8 atmospheres, reaction temperature 5°C, reaction time 30 min.
[0121] b The unit of activity is: 10 6 g / (mol cat.×h).
[0122] c The weight average molecular weight and polydispersity coefficient were determined by high temperature gel permeation chromatography (140°C, with trichlorobenzene as the mobile phase). The unit of weight average molecular weight is: 10 4 g / mol.
[0123] d Melting points were determined by differential scanning calorimetry (DSC).
[0124] e Homogeneous catalyst.
[0125] Note: In Table 1 and the accompanying drawings, A refers to A@UA-Al; AB(1 / 1) refers to AB(1 / 1)@UA-Al, and the same applies to the others; A e Refers to NiA homogeneous catalyst; B e Refers to NiB homogeneous catalyst; AB(1 / 1) e Refers to a homogeneous catalyst of NiA and NiB in a molar ratio of 1:1.
[0126] As can be seen from Table 1 above, the results based on the comparison of the polymerization activity, molecular weight and mechanical properties of the polymers show that, compared with the copolymers catalyzed by homogeneous phase, the polymerization activity is greatly improved when the supported α-diimine nickel heterogeneous catalyst of the present invention is used.
[0127] The mechanical properties of the alloy materials in the polyethylene kettle prepared in Example 1-7, Application Example 9 and Comparative Example 3 were tested. The test results are as follows: Figure 8-11 .
[0128] Figure 8 A comparison chart of the tensile strength of the alloy materials in the polyethylene kettle prepared in Application Examples 1-7, Application Example 9 and Comparative Example 3 of the present invention; Fig. 9 It is a comparison chart of the elongation at break of the alloy materials in the polyethylene kettle prepared in Application Examples 1-7, Application Example 9 and Comparative Example 3 of the present invention; Fig.10 This is a comparison chart of the toughness of the alloy materials in the polyethylene kettle obtained in Application Examples 1-7, Application Example 9 and Comparative Example 3 of the present invention; Fig.11 A comparison chart of Young's modulus of alloy materials in polyethylene kettles prepared in Application Examples 1-7, Application Example 9 and Comparative Example 3 of the present invention;
[0129] from Figure 8-10It can be seen that compared with A+B, A / B and B / A types, the AB type spatial distribution leads to better tensile strength, elongation at break and toughness of the mixture in the reactor. In addition, the AB type heterogeneous catalyst has better mechanical properties than the homogeneous system. Compared with conventional homogeneous catalysts, the mechanical properties (tensile strength, elongation at break, toughness) of the alloy material in the polyethylene kettle prepared by the supported α-diimine nickel heterogeneous catalyst prepared by the present invention are significantly improved.
[0130] Fig.12 This is a comparison diagram of the DSC curves of the alloy materials in the polyethylene kettle obtained in Application Examples 3-6 of the present invention, showing the results of the rheological behavior of the alloy materials in the polyethylene kettle.
[0131] The polyethylene reactor blends of Application Examples 3-6 and Comparative Example 3 were sintered at 25°C and 10 MPa compression pressure for 5 min. Dynamic time sweep tests to measure G' (storage modulus of the melt) were conducted at 160°C, a constant frequency of 10 rad / s, and a strain of 0.2%; Fig.13 It is a comparison chart of the melt stock modulus of the blends in the polyethylene reactor of Application Examples 3-6 of the present invention and Comparative Example 3; Fig.14 Based on Fig.13 Comparison of the obtained modulus improvement rates; Fig.15 Schematic diagram of the structure of AB-type heterogeneous dual-site catalyst at the microscopic scale;
[0132] from Figure 13-15 The results show that the G' value of the blends obtained by heterogeneous catalysts increases significantly less than that of the blends obtained by homogeneous catalyst ethylene polymerization. Among them, the increase caused by the AB type spatial distribution is the smallest, indicating that the three polyolefin components are well mixed together in an entangled manner on a microscopic scale (e.g. Fig.15 In addition, the spatial distribution of the AB type leads to a much higher storage modulus of the melt at low shear compared to the A+B type and AB homogeneous catalysts (as shown in Fig.13 This makes it suitable for the manufacture of thin film products.
[0133] Application Example 12: Polyethylene autoclave alloy is used as a compatibilizer in the recycling of waste HDPE (high-density polyethylene) and PP (polypropylene)
[0134] Waste HDPE and PP were mixed in a ratio of 7:3, and then added with 5wt% AB(1 / 1)@UA-Al heterogeneous catalyst catalyzed polyethylene (PE) in the kettle alloy material, and then pressure tested. The test results are as follows Fig.16 shown.
[0135] Comparative Example 4:
[0136] Waste HDPE and PP were mixed in a ratio of 7:3 and then pressure tested. Fig.16 shown.
[0137] Comparative Example 5:
[0138] Waste HDPE and PP were mixed in a ratio of 7:3, and then 5wt% AB (1 / 1) was added. e The alloy material in the polyethylene (PE) kettle catalyzed by homogeneous catalyst was then pressure tested. The test results are as follows Fig.16 shown.
[0139] Fig.16 It is a strain-stress comparison diagram of Application Example 12 and Comparative Examples 4-5.
[0140] From this Fig.16 It can be seen that compared with Comparative Examples 4 and 5, the copolymer alloy material prepared using the supported heterogeneous dual-site catalyst prepared by the present invention exhibits a greatly increased capacity in its blend compared with the homogeneous system.
[0141] Application Example 13: Using a heterogeneous catalyst to prepare poly(ethylene-aluminum olefin) copolymer alloy materials
[0142] In a 350 ml glass thick-walled pressure vessel, 20 ml of n-heptane solvent and diethylaluminum chloride were placed, and 0.5 mmol of diethylaluminum chloride was slowly added to the system; when no more bubbles were generated in the system, 1.2 ml of CH2Cl2 as a co-catalyst was added; 12 μmol of the catalyst prepared in Example 1-11 was injected into the polymerization system through a syringe, the container was pressurized with ethylene, and stirred continuously at a specific temperature for the required time. The polymer was precipitated and washed with n-hexane. The polymer powder was treated with 2M HCl water, then washed three times with water, and finally washed twice with methanol. The polymer sample was dried in a vacuum oven to constant weight.
[0143] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a heterogeneous dual-site catalyst, It is characterized in that The following steps are involved: S1: adding a metal salt type polar monomer and an organic solvent to a reaction vessel at room temperature under magnetic stirring to dissolve them, adding a co-catalyst, and then adding a mixed solution of two different α-diimine nickel catalysts; S2: After stirring and mixing evenly, let it stand for reaction to obtain; or P1: Add an α-diimine nickel catalyst, a metal salt type polar monomer and an organic solvent into a reaction vessel at room temperature under magnetic stirring to dissolve them; P2: Add a co-catalyst, and then add another α-diimine nickel catalyst, stir and mix evenly, and let it stand to react to obtain; or Q1: At room temperature, under magnetic stirring, add an α-diimine nickel catalyst, a metal salt type polar monomer and an organic solvent into a reaction container to dissolve them, add a co-catalyst, and stir to mix evenly; Q2: Add another α-diimine nickel catalyst and a metal salt type polar monomer, then add an organic solvent to dissolve them, then add a co-catalyst, stir and mix evenly, and let stand to react to obtain; The metal salt type polar monomers are all di(10-undecenoic acid)aluminum chloride; The α-diimine nickel catalyst has a structural formula of or catalyst; the molar ratio of the two different α-diimine nickel catalysts in step S1 is 1:4 to 4:1; the molar ratio of one α-diimine nickel catalyst in step P1 to another α-diimine nickel catalyst in step P2 is 1:4 to 4:1; the molar ratio of one α-diimine nickel catalyst in step Q1 to another α-diimine nickel catalyst in step Q2 is 1:4 to 4:
1.
2. The method for preparing a multiphase dual-site catalyst according to claim 1, It is characterized in that The co-catalyst is one or more of diethylaluminum chloride, methylaluminoxane, ethylaluminum dichloride, triisobutylaluminum and tris(pentafluorophenyl)boron.
3. The method for preparing a multiphase dual-site catalyst according to claim 1, It is characterized in that The organic solvents are one or more of petroleum ether, pentane, hexane, heptane, octane, methylcyclohexane, decalin, cyclohexane, benzene, toluene, xylene, hydrogenated gasoline, dichloromethane, chloroform, chlorobenzene and dichlorobenzene.
4. The method for preparing a multiphase dual-site catalyst according to claim 2, It is characterized in that The co-catalyst is diethylaluminum chloride.
5. The method for preparing a multiphase dual-site catalyst according to claim 1, It is characterized in that The molar ratio of one α-diimine nickel catalyst in step P1 to another α-diimine nickel catalyst in step P2 is 1:4, 1:2, 1:1, 2:1 or 4:
1.
6. The method for preparing a multiphase dual-site catalyst according to claim 1, It is characterized in that The molar ratio of one α-diimine nickel catalyst in step Q1 to another α-diimine nickel catalyst in step Q2 is 1:4, 1:2, 1:1, 2:1 or 4:
1.
7. The method for preparing a heterogeneous dual-site catalyst according to claim 1, It is characterized in that The temperature of the static reaction is 5-25° C., and the time of the static reaction is 4-8 hours.
8. The method for preparing a multiphase dual-site catalyst according to claim 7, It is characterized in that The temperature of the static reaction is 20° C., and the static reaction time is 6 hours.
9. A multiphase dual-site catalyst prepared by the preparation method according to any one of claims 1 to 8.