A method for processing a metal substrate and a material for preparing a vehicle
By adding sodium nitrate or sodium nitrite to the acidic zirconium hydrochloride solution, the problem of insufficient adhesion of the zirconium film on the surface of the metal substrate is solved, the adhesion between the zirconium film and the metal substrate is significantly improved, and the vehicle's life is prolonged. service life and improves the corrosion resistance of the zirconium film.
Patent Information
- Application Number
- CN202310105458.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-02-09
AI Technical Summary
In the existing technology, the zirconium film formed on the surface of the metal substrate does not have strong adhesion and is easy to fall off, resulting in shortened vehicle service life.
Add sodium nitrate or sodium nitrite as an additive to the acidic zirconium hydrochloride solution, and control its concentration between 800 and 1300 ppm to form a zirconium film of nanoscale inorganic films, reduce the formation of manganese compounds, and thereby improve the bond between the zirconium film and the metal substrate. adhesion between.
It significantly improves the adhesion between the zirconium film and the metal substrate, prolongs the service life of the vehicle, and improves the corrosion resistance, acid resistance, and alkali resistance of the zirconium film.
Smart Images

Figure CN116083893B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of vehicle manufacturing, and in particular, to a method for processing a metal substrate and a material for manufacturing a vehicle. Background Art
[0002] During the vehicle manufacturing process, the metal substrate used as the vehicle body generally undergoes processes such as zirconium film coating and electrophoresis treatment, which are generally called painting processes; the metal substrate treated by the painting process is not easy to rust and has a longer service life.
[0003] Among them, the step of coating the zirconium film is one of the steps in the coating process. Generally, the metal substrate is immersed in a zirconium salt solution. The zirconium ions will undergo an electrochemical reaction and a layer of zirconium film will adhere to the surface of the metal substrate. The zirconium film can protect the metal substrate from rust, impact, corrosion, etc., and can increase the service life of the vehicle.
[0004] However, the applicant has found that in the current coating process, after the zirconium film is formed on the surface of the metal substrate, the adhesion between the zirconium film and the metal substrate is easily abnormal due to abnormal shutdown of the conveying equipment, excessively long zirconium immersion time, etc., resulting in the zirconium film falling off the surface of the metal substrate. Summary of the invention
[0005] The embodiments of the present application can provide a method for processing a metal substrate and a material for preparing a vehicle, which can well improve the adhesion between the metal substrate and the zirconium film, and the zirconium film is not easy to fall off the surface of the metal substrate.
[0006] In the first aspect, an embodiment of the present application provides a method for treating a metal substrate, which includes the following steps: immersing the metal substrate in a zirconium salt solution to form a zirconium film, wherein the zirconium salt solution is acidic; and the zirconium salt solution also contains an additive, wherein the additive includes one or both of sodium nitrate and sodium nitrite; and the metal substrate contains manganese, and the mass fraction of manganese is not less than 0.5%.
[0007] In the above technical solution, the metal substrate will undergo an electrochemical reaction in the acidic solution of zirconium salt to form a nano-scale inorganic film, namely, a zirconium film; the zirconium film has strong corrosion resistance, acid resistance, alkali resistance and other properties, and can protect the metal substrate. In addition, the applicant found that the zirconium film on the surface of the metal substrate is easy to fall off because the metal substrate used will inevitably contain manganese. Once the manganese content is too high (generally, the manganese content is not less than 0.5wt%), when the zirconium film is formed, manganese will also participate in the reaction in the form of ions to form loose manganese compounds such as MnF, Mn(OH), and MnOOH that are insoluble in water. These manganese compounds are insoluble in water and are relatively loose, which will affect the adhesion between the zirconium film and the metal substrate, thereby causing the car film to fall off.
[0008] Based on this, the applicant has discovered that if sodium nitrate or sodium nitrite is present in the process of forming the zirconium film, manganese will easily form highly soluble substances such as manganese nitrate, which can effectively remove manganese from the metal substrate, thereby improving the adhesion between the metal substrate and the vehicle film.
[0009] Therefore, adding sodium nitrate or sodium nitrite to the acidic solution of zirconium salt can effectively improve the adhesion between the metal substrate and the zirconium film, so that the zirconium film is not easy to fall off from the surface of the metal substrate.
[0010] In a possible implementation, the concentration of the additive is 800-1300 ppm based on the concentration of sodium ions.
[0011] In the above technical solution, the concentration of the additive is controlled at 800-1300 ppm, which can better ensure that the zirconium film is not easy to fall off from the surface of the metal substrate.
[0012] In a possible implementation, the zirconium salt is a zirconium fluoride salt.
[0013] In the above technical solution, the zirconium salt that meets the above conditions has a faster reaction rate, which is more conducive to improving the coating rate of the zirconium film.
[0014] In a possible implementation, the concentration of the zirconium salt is 0.7 to 1.2 g / L, measured as zirconium ion concentration.
[0015] In a possible implementation, the soaking time in the zirconium salt solution is 3 to 45 minutes; optionally, the soaking time in the zirconium salt solution is 3 to 15 minutes.
[0016] In the above technical solution, controlling the immersion time within the range of 3 to 45 minutes is more conducive to improving the adhesion between the metal substrate and the zirconization film.
[0017] In a possible implementation, the pH value of the zirconium salt solution is 4.0-4.8.
[0018] In a possible implementation, the metal substrate is a cold-rolled plate, and the manganese content of the cold-rolled plate is 0.5% to 3% by weight.
[0019] In the above technical solution, the cold-rolled plate has strong rigidity and is not easily deformed, which is beneficial to improving the strength of the vehicle itself.
[0020] In a possible implementation, after the zirconium film is formed, the metal substrate with the zirconium film attached to the surface is placed in an electrophoresis tank for electrophoresis treatment; the electrophoresis treatment time is 15 to 20 minutes.
[0021] In the above technical solution, after the zirconium film is attached to the surface of the metal substrate, it is electrophoretically treated in an electrophoretic tank to form a car paint film on the surface of the zirconium film. The car paint film can also protect the metal substrate, and the car film can also play an aesthetic role.
[0022] In a possible implementation, a Hy-Lite bacteria detector is used to test the amount of bacteria in the electrophoresis tank, and the amount of bacteria is controlled to be no more than 12.
[0023] In the above technical solution, if the amount of bacteria in the electrophoresis tank is too much, the pH value of the electrophoresis tank will increase. In this way, during the electrophoresis treatment, the thickness of the car paint film formed will be thicker and the structure will be loose, and the adhesion to the zirconium film will be reduced.
[0024] In a second aspect, an embodiment of the present application provides a material for preparing a vehicle, which is obtained by processing the above-mentioned metal substrate processing method.
[0025] In the above technical solution, using the material obtained by the above treatment method, the adhesion between the metal substrate and the zirconium film can be significantly improved, and the zirconium film is not easy to fall off from the surface of the metal substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 A schematic diagram of the adhesion result classification provided in the embodiments of the present application. DETAILED DESCRIPTION
[0028] When producing vehicles such as automobiles and new energy vehicles, most of them use metal substrates such as aluminum alloys and iron alloys to prepare the car body; when using such metal substrates to prepare the car body, it is necessary to adhere a layer of zirconium film to the surface, and then adhere a car paint film to the surface of the zirconium film, so that the metal substrate is not easy to rust.
[0029] However, the applicant has found that when the existing technology is used to form a zirconium film on the surface of a metal substrate, there will be a problem of weak adhesion between the zirconium film and the metal substrate. The zirconium film is easy to fall off from the surface of the metal substrate, so that the car paint film on the surface of the zirconium film will also fall off along with the zirconium film, and the metal substrate will easily rust, and the service life will be affected.
[0030] Based on the above technical problems, the applicant found that the reason why the zirconium film is easy to fall off is that the metal substrate used will inevitably contain manganese. Once the manganese content is too high, manganese will also participate in the reaction when the zirconium film is formed.
[0031] The formation of zirconium film is due to the electrochemical reaction of zirconium salt in acidic solution. The specific reaction mechanism is: HFZr+X+HO→ZrO+X ﹢ +F ﹣ +H ﹢ , where X is the metal ion component of the metal substrate; if X is a metal substrate such as Zn, Mg, Fe, Al, etc., the generated ionic compound is a dense and stable compound, but if X is Mn, it will form loose manganese compounds such as MnF, Mn(OH), MnOOH, etc. that are insoluble in water. These manganese compounds are insoluble in water and are relatively loose, which will affect the adhesion between the zirconium film and the metal substrate, thereby causing the zirconium film to fall off; and once the manganese content in the metal substrate exceeds 0.5%, this phenomenon is particularly obvious.
[0032] Based on this technical problem, the applicant also found that if sodium nitrate or nitrite exists in the process of forming the zirconium film, the Mn 2+ The solubility of zirconium film is reduced to produce substances with high solubility such as manganese nitrate, which will not easily affect the adhesion between the zirconium film and the metal substrate.
[0033] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0034] The following is a detailed description of the method for processing the metal substrate according to the embodiment of the present application.
[0035] S100, forming a zirconium film: immersing the metal substrate in a zirconium salt solution, which is acidic and contains additives such as sodium nitrate and / or sodium nitrite.
[0036] In this step, adding additives such as sodium nitrate and / or sodium nitrite to the acidic solution of zirconium salt can effectively remove manganese in the metal substrate, thereby improving the adhesion between the zirconium film and the metal substrate. In addition, in this step, the concentration of the additive is generally 800 to 1300 ppm in terms of sodium ion concentration, which can better ensure that the zirconium film is not easy to fall off the surface of the metal substrate. The pH of the acidic solution is generally between 4.0 and 4.8, which facilitates the rapid reaction of forming the zirconium film.
[0037] In the actual industrial production process, this step is generally carried out in a zirconization tank, which contains an acidic solution of zirconium salts and substances such as additives. The immersion time of the metal substrate is generally 3 to 45 minutes, specifically 3 to 15 minutes, for example, 4 minutes, 8 minutes, 12 minutes, 20 minutes, 25 minutes, 30 minutes, 40 minutes, etc. If the immersion time is too short, it may lead to incomplete film formation and insufficient corrosion resistance of the zirconization film. If the immersion time is too long, it may lead to uneven film formation or cracks in the film layer, and reduced adhesion. In addition, in the actual industrial production process, additives need to be added continuously to maintain a stable concentration, and when adding additives, the stirring pump in the zirconization tank must be turned off.
[0038] In addition, in this step, the zirconium salt is generally a zirconium fluoride salt. The reaction rate of the zirconium fluoride salt is faster, which is more conducive to improving the coating rate of the zirconium film. In the actual production process, silane and other ingredients are sometimes added to the zirconium fluoride salt. In terms of zirconium ion concentration, the concentration of the zirconium salt is generally between 0.7 and 1.2 g / L, and the concentration of the fluoride ion is generally between 15 and 90 ppm.
[0039] In addition, in this step, the metal substrate is generally a cold-rolled plate, which has strong rigidity and is not easily deformed, which is beneficial to improving the strength of the vehicle itself; and the manganese content in the cold-rolled plate is relatively high. The processing method of the present application is more suitable for cold-rolled plates, especially cold-rolled plates with a manganese content between 0.5wt% and 3.0wt%.
[0040] S200, electrophoresis treatment: placing the metal substrate with the zirconium film attached to the surface in an electrophoresis tank for electrophoresis treatment.
[0041] This step can form a car paint film on the surface of the zirconium film, which can also protect the metal substrate and also be beautiful. The electrophoresis treatment time is generally within the range of 15 to 20 minutes.
[0042] In this step, it is important to pay attention to the amount of bacteria. Use the Hy-Lite bacteria detector to test the amount of bacteria in the electrophoresis tank and control the amount of bacteria to no more than 12. If there are too many bacteria in the electrophoresis tank, the pH value of the electrophoresis tank will increase. During the electrophoresis treatment, the paint film formed will be thicker and looser, and the adhesion to the zirconium film will decrease.
[0043] After the material is processed through the above steps, the adhesion between the metal substrate and the zirconium film will be increased, and the zirconium film will not easily fall off from the surface of the metal substrate, so it can be used to prepare vehicles.
[0044] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0045] Example 1
[0046] This embodiment provides a method for processing a metal substrate, which includes the following steps:
[0047] (1) A cold-rolled steel of model GC270 and containing 0.5 wt% manganese was immersed in a zirconization bath for 3 min to form a zirconization film. The zirconization bath contained a BONDERITE M-NT 1820 solution having a pH value of 4.5 and a concentration of 1.121 g / L in terms of zirconium ion concentration. The zirconization bath also contained sodium nitrate having a concentration of 800 ppm in terms of sodium ion concentration.
[0048] (2) The cold-rolled steel with the zirconium film attached to the surface is placed in an electrophoresis tank for electrophoresis treatment for 16 minutes; the electrophoretic coating in the electrophoresis tank is a cathodic electrophoretic coating, specifically BASF CathoGuard 800-FT25-7820, and the amount of bacteria in the electrophoresis tank is tested using a Hy-Lite bacteria detector to ensure that the amount of bacteria is 10.
[0049] Example 2
[0050] This embodiment provides a method for treating a metal substrate, which has the following main differences compared to Embodiment 1: In step (1), the model of the cold-rolled steel is GC220Y, and the manganese content is 0.8 wt%.
[0051] Example 3
[0052] This embodiment provides a method for treating a metal substrate. Compared with Embodiment 1, the main difference is that in step (1), the model of the cold-rolled steel is GC340, and the manganese content is 1.7 wt%.
[0053] Example 4
[0054] This embodiment provides a method for treating a metal substrate. Compared with Embodiment 1, the main differences are as follows: in step (1), sodium nitrite of the same concentration is used instead of sodium nitrate.
[0055] Example 5
[0056] This embodiment provides a method for treating a metal substrate. Compared with Embodiment 3, the main differences are as follows: in step (1), the concentration of sodium nitrate is 1300 ppm.
[0057] Example 6
[0058] This embodiment provides a method for treating a metal substrate. Compared with Embodiment 1, the main differences are as follows: the zirconium salt is Nippon 9030 (the material contains fluorozirconate and silane).
[0059] Comparative Example 1
[0060] This comparative example provides a method for treating a metal substrate, which has the following main differences compared to Example 1: the zirconization tank does not contain sodium nitrate.
[0061] Comparative Example 2
[0062] This comparative example provides a method for treating a metal substrate, which is different from Example 1 in that sodium chloride of the same concentration is used instead of sodium nitrate.
[0063] Comparative Example 3
[0064] This comparative example provides a method for treating a metal substrate, which is different from Example 6 in that the zirconization tank does not contain sodium nitrate.
[0065] Table 1 shows the main differences between the processing conditions of each embodiment and each comparative example:
[0066] Table 1 Treatment conditions of Examples 1 to 6 and Comparative Examples 1 to 3
[0067]
[0068] Application Examples
[0069] Adhesion tests were performed on the materials in the above examples and comparative examples to obtain detailed adhesion data between the metal substrate and the zirconium film. The test method is as follows:
[0070] According to the requirements of GB / T 5270 and ASTM B 571, use a blade to cut through the electrophoretic coating on the plate to draw a 10*10 grid pattern with a spacing of 1mm, then stick it with 45g / mm tape and tear it off. Figure 1 The medium adhesion result classification diagram is used as the standard, and the test rating results shown in Table 2 are obtained. Specific matters needing attention during the test are:
[0071] (1) Place the specimen on a flat and stable surface to prevent deformation.
[0072] (2) Hold the tool and make the required number of cuts evenly at an appropriate spacing and cutting speed.
[0073] (3) Intersect with the original tangent line at 90° and cut to form a grid pattern.
[0074] (4) Use a soft-bristled brush to brush away debris in a diagonal direction.
[0075] (5) Remove the 75 mm long adhesive tape, place the center of the tape at the center of the grid, and press it flat against the surface with your fingers.
[0076] (6) Within five minutes of application, peel off the tape steadily at a 60° angle within 0.5s or 1s.
[0077] Table 2 Adhesion test rating results of various embodiments and comparative examples
[0078] Group Adhesion test results Placement Test Results Example 1 OK Level 1 Example 2 OK Level 1 Example 3 OK Level 1 Example 4 OK Level 1 Example 5 OK Level 0 Example 6 OK Level 1 Comparative Example 1 NG Level 2 Comparative Example 2 NG Level 2 Comparative Example 3 NG Level 2
[0079] It can be seen from Table 2 that the adhesion between the zirconium film and the metal substrate is significantly improved after the material is treated by the treatment method in this embodiment. The zirconium film can better protect the metal substrate and can be used to prepare vehicles with good performance.
[0080] The above are only embodiments of the present application and are not intended to limit the scope of protection of the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the scope of protection of the present application.
Claims
1. A method for treating a metal substrate, characterized in that: It includes the following steps: The metal substrate is immersed in a zirconium salt solution to form a zirconium film, wherein the zirconium salt solution is acidic; and the zirconium salt solution also contains an additive, wherein the additive includes one or both of sodium nitrate and sodium nitrite; The metal substrate contains manganese, and the mass fraction of manganese is not less than 0.5%; The concentration of the additive is 800-1300 ppm based on the concentration of sodium ions; The time of immersion in the zirconium salt solution is 3 to 45 minutes; The concentration of the zirconium salt is 0.7-1.2 g / L in terms of zirconium ion concentration; The pH value of the zirconium salt solution is 4.0-4.
8.
2. The method for treating a metal substrate according to claim 1, characterized in that: The zirconium salt is a zirconium fluoride salt.
3. The method for treating a metal substrate according to claim 1, characterized in that: The time of immersion in the zirconium salt solution is 3 to 15 minutes.
4. The method for treating a metal substrate according to claim 1, characterized in that: The metal substrate is a cold-rolled plate, and the manganese content of the cold-rolled plate is 0.5% to 3% by weight.
5. The method for treating a metal substrate according to claim 1, characterized in that: After the zirconium film is formed, the metal substrate with the zirconium film attached to the surface is placed in an electrophoresis tank for electrophoresis treatment.
6. The method for treating a metal substrate according to claim 5, characterized in that: The electrophoresis treatment time is 15 to 20 minutes.
7. The method for treating a metal substrate according to claim 5 or 6, characterized in that: The amount of bacteria in the electrophoresis tank was tested using a Hy-Lite bacteria detector to control the amount of bacteria to be no greater than 12.
8. A material for preparing a vehicle, characterized in that: The metal substrate is obtained by being treated by the metal substrate treatment method according to any one of claims 1 to 7.