Metallographic etching agent and metallographic structure display method

Through the combined metallographic etching agent of hydrochloric acid, tert-butylpropane peroxide and ethanol, combined with appropriate oxidation and mechanical polishing steps, the problems of high operational risk and blurred grain boundary display in the existing technology are solved, and clear metallographic etchant is achieved. Phase structure display and stable erosion effect.

CN116083908BActive Publication Date: 2024-10-18WANHUA CHEM GRP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211586876.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-10-18
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

The existing metallographic etching technology has high operational risks when studying nickel-molybdenum alloys, especially the use of highly corrosive substances and complex steps, making it difficult to achieve clear grain boundary display.

Method used

A combined metallographic etchant of hydrochloric acid, tert-butylpropane peroxide and ethanol is used to replace nitric acid, sulfuric acid and other etchants, combined with appropriate oxidation and mechanical polishing steps, to significantly reduce operational risks and improve the clarity of grain boundary display.

Benefits of technology

It realizes the display of metallographic structure with simple operation and good erosion effect. The grain boundary display is clear and the internal grain erosion is small. It has good reproducibility and stability and is suitable for the research of nickel-molybdenum alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003990488560000021
    Figure BDA0003990488560000021
  • Figure BDA0003990488560000051
    Figure BDA0003990488560000051
  • Figure BDA0003990488560000061
    Figure BDA0003990488560000061
Patent Text Reader

Abstract

The invention discloses a metallographic etching agent and a metallographic structure display method. The metallographic etching agent comprises the following components: hydrochloric acid, tert-butyl propane peroxide, ethanol, and water. The invention adopts tert-butyl propane peroxide to replace the etching agent formula such as nitric acid and sulfuric acid, which can corrode the grain boundary, the grain boundary is clearly displayed, it is not easy to be over-corroded, the corrosion to the inside of the grain is small, and the effect of displaying the metallographic structure of the nickel-molybdenum alloy is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a metallographic etching agent, in particular to a metallographic etching agent and a metallographic structure display method, belonging to the technical field of metallographic corrosion. Background Art

[0002] Nickel-molybdenum alloy, as a type of Hastelloy alloy, has the characteristics of high strength, high toughness and high hardness. Adding molybdenum to nickel greatly improves the corrosion resistance in reducing media such as hydrochloric acid and dilute sulfuric acid. It has very important applications in many industries such as chemical industry, petroleum, and metallurgy.

[0003] Therefore, in order to study the properties of nickel-molybdenum alloy, it is necessary to observe the microstructure of nickel-molybdenum alloy, understand the correspondence between its performance and microstructure, and adjust the composition, processing and heat treatment process according to the analysis results to optimize the scope of material use.

[0004] Patent CN110687117A uses different etching solutions and corrodes the metallographic sample in three steps. The metallographic structure is clear and the grain boundaries are easy to distinguish. However, the corrosion process is highly risky, especially the need to heat 98% sulfuric acid to above 90°C, which is difficult and risky to operate.

[0005] Patent CN106644628A uses different etching solutions and corrodes the metallographic sample in two steps, and the obtained metallographic structure is neat and clear with distinct grain boundaries. However, the corrosion process requires the preparation of a highly corrosive aqueous regia solution, which has high operating risks and uses a relatively cumbersome two-step corrosion method. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a metallographic etching agent and a metallographic structure display method, which are suitable for the metallographic research of nickel-molybdenum alloy, easy to operate and have good etching effect.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] A metallographic etching agent comprises the following components: hydrochloric acid, tert-butyl propane peroxide, ethanol and water.

[0009] A metallographic etching agent, comprising the following components:

[0010]

[0011] The concentration of the hydrochloric acid described in the present invention is 36-38wt%.

[0012] The preparation method of the metallographic etching agent of the present invention comprises the following steps: 36-38wt% of hydrochloric acid, tert-butyl propane peroxide, ethanol and deionized water are mixed according to the proportion.

[0013] The invention adopts tert-butyl propane peroxide reagent to replace the etchant formula of nitric acid, sulfuric acid and the like in the prior art, so as to achieve the purpose of corroding the grain boundary and displaying the metallographic structure of the nickel-molybdenum alloy.

[0014] The etchant used in the present invention is tert-butyl propane peroxide reagent, which has the advantages of simple operation and better etching effect compared with reagents such as hydrogen peroxide, sodium peroxide, and peracetic acid. The main reason is that tert-butyl propane peroxide is combined with ethanol in the etching solution, has moderate oxidizing property, and can play a good oxidation role. Hydrogen peroxide and sodium peroxide reagents have strong oxidizing properties themselves, are fully combined with water, and have the characteristics of peroxidation in the oxidation process, resulting in blurred grain boundary corrosion. In addition to having strong oxidizing properties, peracetic acid also contains acetic acid groups, and overall shows the characteristics of peroxidation + strong corrosion, which also results in blurred grain boundaries after etching.

[0015] The invention also provides a metallographic structure display method, comprising the following steps: using the metallographic etching agent of the invention to soak the pre-treated metallographic sample.

[0016] According to the metallographic structure display method, the pretreatment includes the steps of sampling, inlaying, grinding, polishing and the like.

[0017] Sampling refers to taking a part of the sample to be etched for processing, because most of the samples that need to be etched are plates or component materials and cannot be etched as a whole.

[0018] Inlay refers to the process of treating small samples with resin or other materials to facilitate subsequent grinding and polishing operations.

[0019] According to the metallographic structure display method, the polishing is rough grinding and fine grinding using sandpaper.

[0020] According to the metallographic structure display method, the polishing is mechanical polishing using a polishing cloth.

[0021] According to the metallographic structure display method, the immersion time is 1 to 5 minutes, so that the corrosive agent can fully corrode the grain boundaries of the metallographic sample.

[0022] According to the metallographic structure display method, after immersion, the following operations are performed: wash with water to remove the corrosive agent on the surface of the metallographic sample, then rinse with organic alcohol for 10 to 20 seconds, and dry.

[0023] According to the metallographic structure display method, the organic alcohol is preferably one or more of ethanol, methanol, and ethylene glycol that are volatile and have good compatibility with water, and ethanol is more preferred.

[0024] According to the etchant formula, the metallographic specimen used is made of nickel-molybdenum alloy.

[0025] As a preferred solution, a metallographic structure display method comprises the following steps:

[0026] 1) Sampling: Cut and obtain a nickel-molybdenum alloy sample with a size of about 5mm×5mm×2mm

[0027] 2) Mounting: The specimen is mounted by cold mounting; the cold mounting material is phenolic resin or epoxy resin;

[0028] 3) Polishing: The sample is grinded from coarse to fine using a metallographic pre-grinding machine with water sandpaper of different grain sizes until a sample with extremely shallow scratches and a bright surface is obtained;

[0029] 4) Polishing: The sample is mechanically polished. During the polishing process, the polishing spray is sprayed and water is added in a dripping manner until a mirror surface sample is obtained.

[0030] 5) Etching: After the sample is dried, it is directly immersed in the prepared metallographic etching solution, and allowed to stand for 1 to 5 minutes for etching. After etching, the etching solution is immediately rinsed off with water;

[0031] 6) Post-etching treatment: Rinse the sample surface with an organic alcohol solution for 10 to 20 seconds, blow dry with a hair dryer, and then observe the microscopic metallographic structure.

[0032] Compared with the prior art, the present invention has the following advantages:

[0033] (1) The etching agent in the present invention uses tert-butyl propane peroxide reagent instead of nitric acid and sulfuric acid reagents, and the operation risk is low;

[0034] (2) The etchant used in the present invention is tert-butyl propane peroxide, which has the advantages of simple operation and better etching effect compared with hydrogen peroxide, sodium peroxide, peracetic acid and other reagents;

[0035] (3) The etchant has little erosion on the inside of the grain, the grain boundary is clearly displayed, it is not easy to erode excessively, and the erosion effect is good;

[0036] (4) The corrosion reproducibility and stability are good, which is very suitable for the metallographic display of nickel-molybdenum alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1-5 They are respectively microscopic observation pictures of the metallographic structures in the corresponding embodiment 1, embodiment 2, embodiment 3, comparative example 1 and comparative example 2 at a scale of 200 μm. DETAILED DESCRIPTION

[0038] The present invention is further described below through the accompanying drawings and specific embodiments. The embodiments of the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.

[0039] The metallographic structure of the nickel-molybdenum alloy is displayed according to the following steps to obtain the metallographic structure of the nickel-molybdenum alloy under different embodiments and comparative examples. The specific method is:

[0040] 1) Sampling: Cut HB2 nickel-molybdenum alloy specimens with a size of 5 mm × 5 mm × 2 mm and mount the specimens using cold mounting materials;

[0041] 2) Polishing: Place the mounted sample on a metallographic pre-grinding machine and grind it from coarse to fine with 120# water-resistant sandpaper, 400# water-resistant sandpaper, 600# water-resistant sandpaper, 1200# water-resistant sandpaper, and 2000# water-resistant sandpaper, respectively, at a speed of 500r / min; add water to cool it continuously during the grinding process, and when the directions of the scratches are all consistent, one grinding is completed, and the sandpaper is replaced for the next grinding, and the grinding direction is perpendicular to the direction of the previous scratch; repeat the above steps until the grinding with 2000# water-resistant sandpaper is completed, and a sample with extremely shallow scratches and a bright surface is obtained;

[0042] 3) Polishing: The ground sample is mechanically polished (rotation speed 300r / min), with diamond spray polishing agent as the polishing spray, sprayed during the polishing process, and water is injected into the center of the polishing disk in a dripping manner until a mirror surface sample is obtained;

[0043] 4) Etching: After the polished sample is dried with a hair dryer, the sample is directly immersed in the prepared metallographic etching solution, wherein the standing time of Example 1, Example 2 and Example 3 is 3 minutes, 1 minute and 2 minutes respectively, and the standing time of Comparative Example 1 and Comparative Example 2 is 1 minute and 2 minutes respectively for etching, and the etching solution is immediately rinsed off with water after etching;

[0044] 5) Post-etching treatment: Rinse the sample surface with an organic alcohol solution for 20 seconds, rinse off the water, blow dry with a hair dryer, and then observe the microscopic metallographic structure.

[0045] Example 1

[0046] The metallographic etching agent comprises the following components: 36-38% hydrochloric acid, tert-butyl propane peroxide, ethanol and deionized water are prepared according to the mass contents in the following Table 1.

[0047] Table 1

[0048] Components content hydrochloric acid 20% Tert-Butylpropane Peroxide 10% Ethanol 10% water 60%

[0049] Example 2

[0050] The metallographic etching agent comprises the following components: 36-38% hydrochloric acid, tert-butyl propane peroxide, ethanol and deionized water are prepared according to the mass contents in Table 2 below.

[0051] Table 2

[0052]

[0053]

[0054] Example 3

[0055] The metallographic etching agent comprises the following composition: 36-38% hydrochloric acid, tert-butyl propane peroxide, ethanol and deionized water are prepared according to the mass contents in the following Table 3.

[0056] Table 3

[0057] Components content hydrochloric acid 30% Tert-Butylpropane Peroxide 15% Ethanol 15% water 50%

[0058] Comparative Example 1

[0059] The metallographic etching agent comprises the following composition: 36-38% hydrochloric acid, hydrogen peroxide, ethanol and deionized water are prepared according to the mass contents in the following Table 4.

[0060] Table 4

[0061]

[0062]

[0063] Comparative Example 2

[0064] The metallographic etching agent comprises the following composition: 36-38% hydrochloric acid, peracetic acid, ethanol and deionized water are prepared according to the mass contents in the following Table 5.

[0065] Table 5

[0066] Components content hydrochloric acid 30% Peracetic acid 15% Ethanol 15% water 50%

[0067] It can be seen from the metallographic etching photos of Example 2 and Comparative Example 1 that under the same hydrochloric acid content, etching time and other conditions, the metallographic structure of the nickel-molybdenum alloy after etching with the tert-butyl propane formula is clear, and the grains and grain boundaries are clearly displayed, while the grain structure is blurred after etching with the hydrogen peroxide formula, and effective observation cannot be performed. In addition, by comparing the metallographic etching photos of Example 3 and Comparative Example 2, it can also be seen that the effect of etching the nickel-molybdenum alloy with the tert-butyl propane formula is better than that with the peroxyacetic acid formula.

Claims

1. A metallographic etching agent comprising the following components: Hydrochloric acid 20~40wt%; Tert-butyl propane peroxide 5-15wt%; Ethanol 5-15wt%; Water 40~60wt%.

2. The metallographic etching agent according to claim 1, characterized in that: Includes the following components: Hydrochloric acid 25-35wt%; Tert-butyl propane peroxide 8-12wt%; Ethanol 8-12wt%; Water 45~55wt%.

3. The metallographic etching agent according to claim 1, characterized in that: The concentration of the hydrochloric acid is 36-38wt%.

4. A metallographic structure display method, comprising the following steps: The pretreated metallographic sample is immersed in the metallographic etching agent described in any one of claims 1 to 3.

5. The method according to claim 4, characterized in that The pretreatment includes sampling, mounting, grinding and polishing.

6. The method according to claim 4, characterized in that The soaking time is 1 to 5 minutes.

7. The method according to claim 4, characterized in that After soaking, perform the following operations: wash with water to remove the corrosive agent on the surface of the metallographic sample, then rinse with organic alcohol for 10 to 20 seconds, and dry.

8. The method according to claim 7, characterized in that The organic alcohol is selected from one or more of ethanol, methanol and ethylene glycol.

9. The method according to claim 4, characterized in that The metallographic sample is a nickel-molybdenum alloy.

Citation Information

Patent Citations

  • Metallographic corrosive agent for Hastelloy and metallographic structure display method

    CN106644628A

  • Metallographic etching agents for wrought superalloy, and metallographic structure display method for wrought superalloy

    CN110687117A

  • Method for displaying thermal deformation crystal grains of Q690 engineering machinery steel

    CN115308007A