Method for producing strontium titanate microparticles

By using hydrazine or hydrazide compounds to react with organic titanates and strontium compounds under specific conditions, combined with polyols and aminosilane compounds, the problem of time-consuming manufacturing of strontium titanate is solved, and the production of strontium titanate particles with excellent dispersion is achieved. Rapid preparation, suitable for a variety of functional materials.

CN116096677BActive Publication Date: 2024-10-29SAKATA INX
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180056082.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-06
Publication Date
2024-10-29
Estimated Expiration
2041-09-06

AI Technical Summary

Technical Problem

The existing production method of strontium titanate takes a long time, and a simple method is needed to produce strontium titanate particles with excellent dispersion.

Method used

Under the conditions of a pH of 12 or more, a reaction temperature of 150°C or more and 250°C or less, and a reaction time of 0.5 hours or more and 2 hours or less, hydrazine or a hydrazide compound is reacted with an organic titanate and a strontium compound to control the hydrazine Or the molar ratio of the hydrazide compound to the organic titanate is between 10 and 75, and the reaction is carried out in the presence of a polyhydric alcohol and an aminosilane compound.

Benefits of technology

It is possible to produce strontium titanate particles with excellent dispersion under simple conditions. The average particle size is between 10nm and 30nm. They have excellent dispersion and crystallinity and are suitable for applications such as high refractive index materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004113310990000111
    Figure BDA0004113310990000111
Patent Text Reader

Abstract

The present invention provides a method for producing strontium titanate fine particles capable of producing strontium titanate fine particles with excellent dispersibility under simple conditions. The method for producing strontium titanate fine particles comprises a reaction step of reacting an organic titanate with a strontium compound in the presence of a hydrazine or hydrazide compound under the conditions of a pH of 12 or higher, a reaction temperature of 150° C. or higher and 250° C. or lower, and a reaction time of 0.5 hour or higher and 2 hours or lower, wherein the molar ratio of the hydrazine or hydrazide compound to the organic titanate, i.e., the hydrazine or hydrazide compound / organic titanate, is 10 to 75.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing strontium titanate fine particles. Background Art

[0002] Since strontium titanate (SrTiO3) has dielectric properties, thermoelectric properties, photocatalytic ability, high refractive index property, etc., it is expected to be popularized as a functional material in various applications.

[0003] For example, Patent Document 1 discloses that strontium titanate having an average particle diameter of 50 nm or less, an average aspect ratio of 1.0 to 1.2, and a refractive index of 1.8 to 2.6 has a high refractive index property. In addition, Patent Document 1 discloses that when using strontium titanate as a component for imparting a high refractive index property, high dispersibility in which it does not aggregate in a coating film is required.

[0004] In addition, as a method for manufacturing strontium titanate, for example, Patent Document 2 discloses a method for manufacturing strontium titanate by heat-treating titanium bis(ammoniumlactate)dihydroxide (TALH) and strontium hydroxide in a constant temperature bath at 200°C for 24 hours in the presence of oleic acid and hydrazine.

[0005] However, in the method described in Patent Document 2, it takes too much time to manufacture strontium titanate, so there is a need for a method that can be manufactured more simply.

[0006] Prior Art Documents

[0007] Patent Documents

[0008] Patent Document 1: International Publication No. 2011 / 004750

[0009] Patent Document 2: Japanese Patent Application Laid-Open No. 2011-068500 Summary of the Invention

[0010] Problems to be Solved by the Invention

[0011] An object of the present invention is to provide a method for manufacturing strontium titanate fine particles that can manufacture strontium titanate fine particles having excellent dispersibility under simple conditions.

[0012] The inventors of the present invention conducted in-depth research on the method for manufacturing strontium titanate fine particles, and as a result, found that by containing a specific amount of hydrazine or hydrazide compound and reacting an organic titanate with a strontium compound under specified conditions (temperature and reaction time), strontium titanate fine particles having excellent dispersibility can be manufactured in a shorter reaction time than in the past.

[0013] Means for Solving the Problems

[0014] The present invention is a method for producing strontium titanate particles, which includes a reaction step of reacting an organic titanate with a strontium compound in the presence of a hydrazine or hydrazide compound and under the conditions of a pH of 12 or higher, a reaction temperature of 150°C or higher and 250°C or lower, and a reaction time of 0.5 hour or higher and 2 hours or lower, wherein the molar ratio of the hydrazine or hydrazide compound to the organic titanate (hydrazine or hydrazide compound / organic titanate) is 10 to 75.

[0015] The method for producing strontium titanate fine particles of the present invention preferably comprises a mixing step of mixing an organic titanate and a hydrazine or hydrazide compound in a solvent to obtain a mixed solution, an adjusting step of adjusting the pH of the mixed solution to 12 or more, and the reaction step.

[0016] In the method for producing strontium titanate of the present invention, the reaction step is preferably carried out in the presence of a polyol. The polyol is preferably ethylene glycol.

[0017] In addition, the organic titanate is preferably titanium lactate.

[0018] In addition, the strontium compound is preferably at least one selected from strontium acetate and strontium formate.

[0019] In addition, the above reaction step is preferably performed in the presence of an aminosilane compound.

[0020] In addition, the aminosilane compound is preferably 3-aminopropyltriethoxysilane.

[0021] Effects of the Invention

[0022] The method for producing strontium titanate fine particles of the present invention can produce strontium titanate fine particles having excellent dispersibility under simple conditions. DETAILED DESCRIPTION

[0023] The present invention is a method for producing strontium titanate particles, which includes a reaction step of reacting an organic titanate with a strontium compound in the presence of a hydrazine or hydrazide compound and under the conditions of a pH of 12 or higher, a reaction temperature of 150°C or higher and 250°C or lower, and a reaction time of 0.5 hour or higher and 2 hours or lower, wherein the molar ratio of the hydrazine or hydrazide compound to the organic titanate (hydrazine or hydrazide compound / organic titanate) is 10 to 75.

[0024] First, various materials used in the method for producing strontium titanate fine particles of the present invention will be described.

[0025] (Organic Titanate)

[0026] Examples of the organic titanate include tetraethyl titanate, tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetra(2-ethylhexyl) titanate and polymers thereof, acetyl titanium titanate, polyacetylacetonate titanium, glycine octyl titanium, titanium lactate, ethyl titanium lactate, triethanolamine titanium (titanium triethanolaminate), titanium chelates such as phosphate titanium complexes, and the like.

[0027] Among them, titanium lactate is preferred from the viewpoint of hydrophilicity.

[0028] (Hydrazine or hydrazide compound)

[0029] Examples of the hydrazide compound include 1-monomethylhydrazine, 1,1-dimethylhydrazine, 1-ethyl-2-methylhydrazine, adipic acid dihydrazide, oxalic acid dihydrazide, malonic acid dihydrazide, succinic acid dihydrazide, glutaric acid dihydrazide, isophthalic acid dihydrazide, sebacic acid dihydrazide, maleic acid dihydrazide, fumaric acid dihydrazide, and itaconic acid dihydrazide.

[0030] Among them, hydrazine is preferred because it is relatively easy to handle and has an excellent effect of controlling the shape of the obtained strontium titanate fine particles.

[0031] The above-mentioned hydrazine or hydrazide compound may be in a hydrogenated state.

[0032] The molar ratio of the content of the hydrazine or hydrazide compound to the organic titanate (hydrazine or hydrazide compound / organic titanate) is 10 to 75, preferably 30 to 65.

[0033] By setting the content within the above range, the shape of the obtained strontium titanate fine particles can be controlled.

[0034] (Strontium compounds)

[0035] Examples of the strontium compound include strontium nitrate, strontium hydroxide, strontium carbonate, strontium peroxide, strontium formate, strontium acetate, strontium lactate, strontium oxalate, strontium chloride, strontium fluoride, strontium iodide, strontium bromide, strontium chlorate, strontium iodate, strontium perchlorate, etc. These compounds may also be used as hydrates.

[0036] Among them, from the viewpoint of hydrophilicity, at least one selected from strontium acetate and strontium formate is preferred, and strontium acetate is more preferred.

[0037] The content of the strontium compound is preferably 1.0 or more in terms of a molar ratio (strontium compound / organic titanate) relative to the organic titanate.

[0038] By setting it in the said range, the progress of crystallization can be controlled appropriately.

[0039] From the viewpoint of reducing the cost of raw materials, the molar ratio (strontium compound / organic titanate) is more preferably 2.0 or less.

[0040] (Solvent)

[0041] As the solvent used in the method for producing strontium titanate fine particles of the present invention, ion-exchanged water is preferably used.

[0042] In addition, the above-mentioned solvent preferably contains a polyol.

[0043] Examples of the polyol include diols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, trimethylene glycol, butanediol, pentanediol, hexanediol, heptanediol, nonanediol, decanediol and neopentyl glycol; and trivalent or higher polyols such as glycerol, trimethylolpropane and pentaerythritol.

[0044] Among them, from the viewpoint of adjusting the particle size of the obtained strontium titanate fine particles and maintaining appropriate dispersibility in the reaction system, at least one selected from ethylene glycol, propylene glycol, diethylene glycol, and 1,3-propylene glycol is preferred, and ethylene glycol is more preferred.

[0045] The content of the polyol is preferably 1 to 20% by mass, more preferably 3 to 15% by mass, and even more preferably 7 to 12% by mass, based on the total amount of the solvent.

[0046] (pH adjuster)

[0047] In the method for producing strontium titanate fine particles of the present invention, it is preferred to adjust the pH using a pH adjuster.

[0048] Examples of the pH adjuster include lithium hydroxide, sodium hydroxide, potassium hydroxide, calcium hydroxide, and ammonium hydroxide.

[0049] Among them, potassium hydroxide is preferred from the viewpoint of solubility in the above solvents.

[0050] When adjusting the pH, the pH is set to 12 or more from the viewpoint of controlling the reaction rate and the shape of the obtained strontium titanate fine particles.

[0051] The pH is preferably 12.5 or higher, more preferably 13 or higher, and further preferably 13.5 or higher.

[0052] The content of the pH adjuster is not limited, and can be appropriately added according to the target pH.

[0053] (Aminosilane compound)

[0054] The above reaction step is preferably performed in the presence of an aminosilane compound.

[0055] By carrying out the above-mentioned reaction step in the presence of an aminosilane compound, the average particle size of the obtained strontium titanate fine particles can be further reduced, and better dispersibility can be imparted.

[0056] Examples of the aminosilane compound include 3-aminopropyltrimethoxysilane, 3-aminopropylethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane.

[0057] Among them, 3-aminopropyltriethoxysilane is preferred.

[0058] The content of the aminosilane compound is preferably 0.003 to 0.025, more preferably 0.004 to 0.019, and even more preferably 0.007 to 0.015, in terms of molar ratio relative to the hydrazine or hydrazide compound (aminosilane compound / hydrazine or hydrazide compound).

[0059] (other)

[0060] In the method for producing strontium titanate fine particles of the present invention, no amphiphilic compound may be added.

[0061] In the conventional method for producing strontium titanate fine particles, the particle size and shape are highly controlled by carrying out the reaction in the presence of an amphiphilic compound, thereby imparting dispersibility to the particles.

[0062] On the other hand, in the method for producing strontium titanate fine particles of the present invention, if the amphiphilic compound is added, it is not uniformly dispersed in the system, resulting in an increase in the average particle size of the obtained strontium titanate fine particles.

[0063] As the above-mentioned amphiphilic compounds, for example, there can be mentioned: saturated fatty acids such as propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, behenic acid, and tetradecanoic acid; and unsaturated fatty acids such as α-linolenic acid, octadecatetraenoic acid, eicosapentaenoic acid, docosahexaenoic acid, linoleic acid, γ-linolenic acid, dihomo-γ-linolenic acid, arachidonic acid, oleic acid, elaidic acid, erucic acid, and nervonic acid.

[0064] (Manufacturing method)

[0065] The method for producing strontium titanate fine particles of the present invention comprises a reaction step of reacting an organic titanate with a strontium compound in the presence of hydrazine or a hydrazide compound at a pH of 12 or higher, a reaction temperature of 150° C. to 250° C., and a reaction time of 0.5 hour to 2 hours.

[0066] The method for producing strontium titanate fine particles of the present invention preferably includes, for example, a mixing step of mixing an organic titanate and a hydrazine or hydrazide compound in a solvent to obtain a mixed solution, an adjusting step of adjusting the pH of the mixed solution to 12 or more, and the reaction step.

[0067] The mixing step is a step of adding the organic titanate and the hydrazine or hydrazide compound to a solvent.

[0068] It is presumed that hydrazine is coordinated to the organic titanate through the above-mentioned mixing step.

[0069] In the mixing step, the method of adding the various materials is not particularly limited, and the materials may be added or stirred by a known method.

[0070] In the adjustment step, pH is adjusted, thereby enabling the reaction rate and the shape of the obtained strontium titanate fine particles to be appropriately controlled.

[0071] Furthermore, by controlling the increase in the average particle size of the organic titanate coordinated with hydrazine through the mixing step, the average particle size of the obtained strontium titanate fine particles can be controlled within an appropriate range.

[0072] In addition, the pH is preferably adjusted using the above-mentioned pH adjuster.

[0073] When the aminosilane compound is added, it is preferably added together with the pH adjuster in the adjustment step.

[0074] For strontium titanate particles, on the one hand, if a large amount of water is present, the crystal growth becomes faster; on the other hand, if the hydrophobicity of the solvent becomes higher, since the surface of the strontium titanate particles is hydrophilic, aggregation is promoted.

[0075] On the other hand, since the above-mentioned polyol has hydrophilicity and has the effect of inhibiting crystal growth, it is preferably added in the above-mentioned preparation step.

[0076] In the above-mentioned adjustment step, the method of adding various materials is not particularly limited, and addition, stirring, etc. can be performed by a known method.

[0077] In the reaction step, the organic titanate and the strontium compound are reacted under the conditions of pH 12 or higher, reaction temperature 150° C. or higher and 250° C. or lower, and reaction time 0.5 hour or higher and 2 hours or lower.

[0078] The reaction temperature is 150°C or higher and 250°C or lower.

[0079] If the reaction temperature is lower than 150° C., the reaction does not proceed and the target strontium titanate fine particles may not be obtained. If the reaction temperature exceeds 250° C., the reaction efficiency decreases and the obtained strontium titanate fine particles become larger and have lower dispersibility.

[0080] The reaction temperature is preferably 180 to 250°C, more preferably 200 to 240°C.

[0081] The reaction time is 0.5 hours to 2 hours.

[0082] If the reaction temperature is lower than 150° C., the reaction does not proceed and the target strontium titanate fine particles cannot be obtained. If the reaction temperature exceeds 250° C., the reaction efficiency decreases and the obtained strontium titanate fine particles become larger and have lower dispersibility.

[0083] The above reaction time is preferably 1 to 2 hours.

[0084] The pressure during the reaction may be, for example, approximately 2 to 5 MPa, and there is no need to apply a pressure exceeding 10 MPa.

[0085] The method for carrying out the reaction step is not particularly limited as long as it is a method that satisfies the above conditions.

[0086] For example, a pressure reaction vessel or the like may be used.

[0087] (Strontium titanate particles)

[0088] The strontium titanate fine particles obtained by the method for producing strontium titanate fine particles of the present invention have the following properties.

[0089] The strontium titanate fine particles are preferably spherical in shape.

[0090] Here, the so-called spherical shape includes not only a sphere but also an ellipsoid, a cylinder, a straw bag shape (a shape in which the corners of a cylinder are rounded), and the like.

[0091] Specifically, it means that the circularity of the strontium titanate fine particles is 0.900 to 1.000.

[0092] The shape of the strontium titanate fine particles can be confirmed by, for example, observing them with a transmission electron microscope ("JEM-1011" manufactured by JEOL Ltd.) at a magnification of 300,000 times.

[0093] In addition, as the circularity of the strontium titanate particles, if the area of ​​the particles in the image taken by a transmission electron microscope is S and the perimeter is L, the circularity can be expressed as: 4πS / L 2 to calculate.

[0094] The circularity is an average value of particles appearing in an image taken with a transmission electron microscope, excluding particles having a special shape that is clearly different from the spherical shape.

[0095] The average particle size of the strontium titanate fine particles is preferably 10 nm to 30 nm, and more preferably 14 nm to 25 nm.

[0096] By having such an average particle size, it is possible to have excellent dispersibility.

[0097] The above average particle size refers to the average particle size (D50) obtained by dissolving strontium titanate particles in methanol to obtain a dispersion, placing the obtained dispersion into a measuring element (measuring cell), and measuring it using a laser diffraction / scattering particle size distribution measuring instrument (manufactured by Nikkiso Co., Ltd., “Microtrack MT 3300EXII”).

[0098] The strontium titanate fine particles have excellent dispersibility.

[0099] Here, the so-called dispersibility can be judged as follows: after dissolving 50 mg of strontium titanate particles in 50 mL of methanol to obtain a dispersion, the obtained dispersion is placed in a spiral tube bottle and black paper is set on the back. When visually confirming the state of the dispersion, the dispersibility is judged by whether white turbidity occurs. In the case of no white turbidity, it can be evaluated as having excellent dispersibility, for example, it can be applied to high refractive index materials, etc.

[0100] The strontium titanate fine particles preferably have good crystallinity.

[0101] In addition, regarding the crystallinity of the above-mentioned strontium titanate particles, if the crystallite size calculated by the X-ray diffraction device is the same as the particle size observed by the transmission electron microscope [the ratio of the particle size (particle size observed by the transmission electron microscope / crystallite size calculated by the X-ray diffraction device) is 0.9 to 1.0], then the crystallinity is judged to be good. If the ratio is smaller or no crystallinity is confirmed, it is judged to be poor.

[0102] In the strontium titanate fine particles, the content of the hydrazine or hydrazide compound is preferably 0.1% by mass to 60% by mass based on the strontium titanate fine particles.

[0103] Based on such a content, dispersibility becomes good.

[0104] Example

[0105] The present invention will be described in further detail below by giving examples, but the present invention is not limited to these examples. In addition, unless otherwise specified, "%" means "mass %", and "part" means "mass part".

[0106] The materials used in Examples and Comparative Examples are as follows.

[0107] (Organic Titanate)

[0108] Titanium lactate (ORGATIX TC-310, component concentration 44 wt%, manufactured by Matmoto Fine Chemical Co., Ltd.)

[0109] Phosphate ester titanium complex (ORGATIX TC-1040, component concentration 75 wt%, manufactured by Matmoto Fine Chemical Co., Ltd.)

[0110] (Hydrazine or hydrazide compound)

[0111] Hydrazine hydrate (manufactured by NIPPON CARBIDE INDUSTRIES CO., INC.)

[0112] (Strontium compounds)

[0113] Strontium acetate hemihydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0114] Strontium formate dihydrate

[0115] (Solvent)

[0116] Ethylene glycol

[0117] Propylene glycol

[0118] Purified water (ion exchange water)

[0119] (pH adjuster)

[0120] Potassium hydroxide

[0121] (Aminosilane compound)

[0122] 3-Aminopropyltriethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0123] (Example 1)

[0124] 3 g of purified water and 3.0 g of hydrazine hydrate (manufactured by Nippon Carbide Industries Co., Ltd.) were added to 0.584 g of titanium lactate (ORGATIX TC-310, component concentration 44% by weight, manufactured by Matsumoto Fine Chemical Co., Ltd.) to obtain a yellow transparent solution.

[0125] Next, a solution prepared with 0.48 g of potassium hydroxide, 0.432 g of ethylene glycol, and 5.088 g of purified water was added to the yellow transparent solution to obtain a white turbid solution.

[0126] Then, 0.429 g of strontium acetate hemihydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the obtained turbid solution, and stirred at room temperature for 30 minutes to obtain a transparent solution. The obtained transparent solution was placed in a pressure reaction vessel and reacted at 230° C. for 1 hour. In addition, the pressure was about 2.8 MPa.

[0127] The solution containing the reactants was centrifuged (model name: SIGMA 3-30KS, condition: 15000 rpm, 5 minutes) to allow the microparticles to settle, thereby separating and purifying (refining) the microparticles from the unreacted products. A redispersed solution of the microparticles was prepared with purified water, and centrifuged. The operation of allowing the microparticles to settle was repeated 3 times to complete the separation and purification.

[0128] The obtained fine particles were recovered and observed using an X-ray diffraction apparatus ("MiniFlex600-C" manufactured by Rigaku Corporation), and it was confirmed that they were fine particles of strontium titanate.

[0129] (Examples 2 to 8, Comparative Examples 1 to 6)

[0130] Strontium titanate fine particles were produced in the same manner as in Example except that the blending amounts of various materials and the reaction conditions were changed as shown in Table 1.

[0131] In addition, in Examples 5 and 6, 3-aminopropyltriethoxysilane was added together with the pH adjuster (potassium hydroxide).

[0132] The obtained fine particles were recovered and observed using an X-ray diffraction apparatus ("MiniFlex600-C" manufactured by Rigaku Corporation). As a result, it was confirmed that the fine particles in Examples 2 to 8 and Comparative Example 4 were strontium titanate fine particles.

[0133] On the other hand, in Comparative Examples 1 to 3, 5, and 6, the reaction did not proceed, and strontium titanate fine particles were not obtained.

[0134] <Evaluation method>

[0135] (Particle shape)

[0136] The fine particles obtained in Examples and Comparative Examples were recovered and observed with a transmission electron microscope ("JEM-1011" manufactured by JEOL Ltd.) at a magnification of 300,000 times to confirm the particle shape.

[0137] The confirmed microparticles having a circularity of 0.900 to 1.000 were evaluated as spherical.

[0138] (Crystallinity)

[0139] The fine particles obtained in Examples and Comparative Examples were observed using a transmission electron microscope ("JEM-1011" manufactured by JEOL Ltd.) and an X-ray diffraction apparatus ("MiniFlex600-C" manufactured by Rigaku Corporation), and evaluated according to the following criteria.

[0140] 0: The ratio of the crystallite size calculated by an X-ray diffraction device to the particle size observed by a transmission electron microscope is 0.9 to 1.0;

[0141] △: The ratio of the crystallite size calculated by an X-ray diffraction device to the particle size observed by a transmission electron microscope is less than 0.9;

[0142] ×: No crystals were generated.

[0143] (Average particle size)

[0144] 50 mg of the fine particles obtained in Examples and Comparative Examples were dissolved in 50 mL of methanol to obtain a dispersion.

[0145] The obtained dispersion was placed in a measuring cell, and the average particle size (D50) was measured using a laser diffraction / scattering particle size distribution measuring instrument ("microtrack MT 3300EXII" manufactured by Nikkiso Co., Ltd.).

[0146] (Dispersion)

[0147] 50 mg of the fine particles obtained in Examples and Comparative Examples were dissolved in 50 mL of methanol to obtain a dispersion.

[0148] The obtained dispersion was put into a screw bottle, black paper was placed on the back, the state of the dispersion was visually checked, and the evaluation was performed according to the following criteria.

[0149] ○: The obtained dispersion was a transparent solution.

[0150] ×: The obtained dispersion liquid was a cloudy solution.

[0151]

[0152] The strontium titanate fine particles obtained in the examples had a spherical particle shape and an average particle diameter of 14 nm to 30 nm, and were confirmed to have excellent crystallinity and dispersibility.

[0153] In particular, in Examples 5 and 6 in which 3-aminopropyltriethoxysilane was added, strontium titanate fine particles having a small average particle size and excellent dispersibility were obtained.

[0154] In Example 7 using a phosphate titanium complex and Example 8 using propylene glycol as a solvent, the results showed that the transparency of the dispersion was slightly lower than that of the other examples, and the dispersibility was slightly lower than that of the other examples.

[0155] On the other hand, in Comparative Examples 1 to 3, 5, and 6, the reaction did not proceed, and strontium titanate fine particles were not obtained.

[0156] In addition, the fine particles obtained in Comparative Examples 1 to 3 (in which hydrazine or hydrazide compound was not contained or the added amount was outside the prescribed range) had a large average particle size and poor dispersibility (the dispersion was turbid).

[0157] In addition, the strontium titanate fine particles obtained in Comparative Example 4, in which the reaction temperature was not within the prescribed range, had insufficient crystallinity.

[0158] In addition, the fine particles obtained in Comparative Example 5 in which the reaction time was too long had a large average particle size and poor dispersibility (the dispersion was turbid).

[0159] In Comparative Example 6, in which the reaction time was long and the pH was low, the reaction did not proceed and fine particles were not obtained.

[0160] Industrial Applicability

[0161] The method for producing strontium titanate particles of the present invention is useful in that it is possible to obtain strontium titanate particles that can be used as functional materials such as high refractive index agents, thermoelectric conversion materials, photocatalysts, ion conductive materials, ferroelectric materials, magnetic materials, catalyst materials, oxygen electrode materials, piezoelectric materials, thermoelectric materials, nonlinear optical materials, and fillers.

Claims

1. A method for producing strontium titanate particles, comprising: A step of reacting an organic titanate with a strontium compound in the presence of hydrazine or a hydrazide compound under the conditions of pH 12 or higher, reaction temperature 150° C. or higher and 250° C. or lower, and reaction time 0.5 hour or higher and 2 hours or lower, and The molar ratio of the hydrazine or hydrazide compound to the organic titanate, that is, the hydrazine or hydrazide compound / organic titanate, is 10 to 75, The reaction step is performed in the presence of an aminosilane compound.

2. The method for producing strontium titanate particles according to claim 1, comprising: A mixing step of mixing an organic titanate and a hydrazine or hydrazide compound in a solvent to obtain a mixed solution; A step of adjusting the pH of the mixed solution to 12 or above; and The reaction process.

3. The method for producing strontium titanate fine particles according to claim 1 or 2, wherein: The reaction step is carried out in the presence of a polyol.

4. The method for producing strontium titanate fine particles according to claim 3, wherein: The polyol is ethylene glycol.

5. The method for producing strontium titanate fine particles according to claim 1 or 2, wherein: The organic titanate is titanium lactate.

6. The method for producing strontium titanate fine particles according to claim 1 or 2, wherein: The strontium compound is at least one selected from strontium acetate and strontium formate.

7. The method for producing strontium titanate fine particles according to claim 1 or 2, wherein: The aminosilane compound is 3-aminopropyltriethoxysilane.

Citation Information

Patent Citations

  • Method for producing multiple oxide nanoparticles

    JP2011068500A

  • High-refractive index powder and production method and application of same

    WO2011004750A1