A slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst and its preparation method and application

By in-situ growth of Na+-doped low conductivity band amorphous MnO2 on slag-based Fe2O3, a slag-based Fe2O3/MnO2 composite photo-Fenton catalyst with high oxidation and reduction performance was constructed, which solved the small surface area and insufficient light absorption capacity of slag-based Fe2O3. solve the problem, achieve efficient removal of ciprofloxacin hydrochloride and Cr(VI), and reduce environmental pollution of industrial waste.

CN116099544BActive Publication Date: 2024-10-29GUANGXI UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310114117.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-15
Publication Date
2024-10-29
Estimated Expiration
2043-02-15

AI Technical Summary

Technical Problem

The slag-based Fe2O3 in the existing photo-Fenton catalyst has a small specific surface area, insufficient photoreduction ability, limited light absorption capacity, and easy recombination of photogenerated electrons and holes, resulting in low reaction efficiency.

Method used

Slag-based Fe2O3 was prepared by oxidative roasting, and Na+-doped low-conductivity band amorphous MnO2 was grown in situ through impregnation adsorption and persulfate oxidation methods to construct a slag-based Fe2O3/MnO2 composite photo-Fenton catalyst with high oxidation and reduction properties. , enhance its specific surface area and light absorption capacity, and improve electron migration efficiency.

Benefits of technology

The photocatalytic activity of the catalyst is significantly improved, the degradation rate of ciprofloxacin hydrochloride reaches more than 81.9%, and the Cr(VI) removal rate reaches more than 85.2%, which reduces the harm of composite pollutants to the environment, and the preparation method is simple and low-cost. Suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004077860380000011
    Figure HDA0004077860380000011
  • Figure HDA0004077860380000012
    Figure HDA0004077860380000012
  • Figure HDA0004077860380000021
    Figure HDA0004077860380000021
Patent Text Reader

Abstract

The present invention discloses a slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst and a preparation method and application thereof, and belongs to the technical field of wastewater treatment. The present invention prepares slag-based Fe2O3 by oxidative roasting of manganese slag, and in-situ grows Na2O3 by impregnation adsorption and persulfate oxidation. + Doped low-conduction band amorphous MnO2 is used to construct a direct Z-type composite photo-Fenton catalyst with oxidation and reduction properties. The preparation method of the catalyst is as follows: (1) crushing manganese slag, oxidizing and roasting the crushed manganese slag to obtain slag-based Fe2O3; (2) adding the slag-based Fe2O3 to a manganese sulfate solution for impregnation and adsorption, filtering, and obtaining filter residue I; (3) adding the filter residue I to a NaCl aqueous solution, and adding a persulfate solution, stirring, and obtaining a suspension; (4) vigorously stirring the suspension, filtering, and drying the obtained filter residue II to obtain a composite catalyst. The catalyst can be used for the simultaneous removal of ciprofloxacin hydrochloride and Cr(VI), and has a good application value for the degradation and removal of composite pollutants.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wastewater treatment, and specifically relates to a slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst and a preparation method and application thereof. Background Art

[0002] Antibiotics and heavy metals have become one of the typical types of complex pollution, mainly from the discharge of livestock and poultry manure, agricultural use of manure, sewage irrigation, etc. Among them, hexavalent chromium is the most toxic, more than 100 times that of trivalent chromium. Excessive chromium discharged from wastewater can cause soil pollution, plant inactivation and death, and even cause cancer after being absorbed by the human body. In the complex system, antibiotics and heavy metals have a complex existence form, which produces different degrees of joint toxic effects on biological organisms, such as additive, synergistic, and antagonistic effects.

[0003] Photocatalytic technology has been proven to be an effective technology for remediating wastewater containing the above pollutants due to its advantages of high efficiency, simplicity, environmental protection and economy. It can achieve complete mineralization of organic pollutants under ambient temperature and atmospheric pressure conditions, while producing low-toxic byproducts. If sufficient light energy is provided, electrons and holes can be generated at the same time, so the photocatalyst can achieve oxidation and reduction simultaneously in one reaction system. Among them, the photo-Fenton method, as a prominent method in environmental remediation, has attracted more and more attention. Photogenerated electrons, Fe 2+ / Fe 3+ The H2O2 in the Fenton system can reduce heavy metals to low-valent states, and the free radicals ·OH, ·O2 - and h + It tends to degrade organic pollutants, thereby achieving the purpose of removing two pollutants at the same time.

[0004] Hematite (α-Fe2O3) is a chemically stable, non-toxic, low-cost n-type semiconductor material. It is widely used in photocatalysis and photo-Fenton systems due to its narrow bandgap (Eg = 2.2 eV), good absorption characteristics for visible light, and chemical stability in aqueous solutions with a pH greater than 3. In particular, its VB edge is at a low position, and it exhibits high oxidation performance under sunlight, making it easier to degrade organic pollutants. However, its conduction band (CB) potential is weak, so part of the energy in the photocatalytic reaction cannot be fully utilized and its reducibility is poor. In addition, photogenerated electron and hole pairs are easy to recombine, which seriously reduces the reaction efficiency. In order to overcome these shortcomings, many methods have been adopted to solve these problems. The construction of Z-type photocatalysts has attracted much attention for improving the separation of photogenerated charges and extending the electron lifetime, as well as the ability to inhibit the interfacial recombination of photogenerated charges. Improving suitable bandgap semiconductors with sufficient valence band (VB) and conduction band (CB) is crucial for orderly photocatalytic degradation under solar illumination.

[0005] MnO2 is a transition metal oxide with diverse structures. Due to its low price, abundant content, excellent valence adjustability and crystal structure controllability, it is widely used in the fields of thermal catalysis, electrocatalysis and photocatalysis. MnO2 with different crystal forms and surface structures prepared by different synthesis processes show greatly different surface oxygen vacancy content and catalytic performance. α-MnO2 has the highest catalytic activity. Its commonly used preparation methods include sol-gel method, hydrothermal method, reduction method and persulfate oxidation method. Among them, the persulfate oxidation method is widely used because of its mild reaction conditions and can prepare manganese oxides with adjustable band gap width by changing the type of alkali metal ions in the solution. Based on this, it is a very meaningful study to prepare MnO2 nanoparticles with low reduction potential anchored on α-Fe2O3 by a suitable method to improve its photocatalytic activity.

[0006] Manganese slag is an industrial waste produced in the process of producing manganese sulfate by acid leaching using pyrolusite and pyrite as the main raw materials. Its main components are SiO2 and jarovanadium slag. If it is not effectively treated, it will cause serious harm to the ecosystem. The main components of the slag after oxidative roasting are SiO2 and Fe2O3. Metal cations can enter the slag through ion exchange, impregnation or adsorption on the slag surface to improve the catalytic performance of the catalyst. Na in the solution + It can effectively regulate the crystal growth of MnO2.

[0007] Therefore, the present invention uses manganese slag as the main raw material to prepare slag-based Fe2O3 compounds by oxidative roasting, and in-situ grows Na +Doped low-conduction band amorphous MnO2 was used to construct a direct Z-type photo-Fenton catalyst with high oxidation and reduction performance for simultaneous oxidation and degradation of ciprofloxacin hydrochloride and reduction of Cr(VI). This will open up new ways for the resource utilization of industrial waste and environmental remediation using inexhaustible solar energy. Summary of the invention

[0008] In view of the above problems, the present invention provides a slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst and its preparation method and application. Manganese slag is used as the main raw material to prepare slag-based Fe2O3 compounds by oxidative roasting, and Na2O3 is grown in situ by impregnation adsorption and persulfate oxidation. + Doped low-conduction band amorphous MnO2 was used to construct a direct Z-type photo-Fenton catalyst with high oxidation and reduction properties, which was applied to the photo-Fenton efficient degradation of ciprofloxacin hydrochloride and reduction of Cr(VI), solving the problems of small specific surface area of ​​slag-based Fe2O3, insufficient photoreduction ability, limited light absorption capacity, and easy recombination of photogenerated electron-hole pairs.

[0009] The present invention is achieved through the following technical solutions:

[0010] A slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst is prepared by oxidative roasting of manganese slag to prepare slag-based Fe2O3, and Na2O3 is grown in situ by impregnation adsorption and persulfate oxidation. + Doped low-conduction band amorphous MnO2 was used to construct a direct Z-type slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst with oxidation and reduction properties.

[0011] The specific surface area of ​​the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst of the present invention is 55-56 m 2 / g, pore volume is 0.10~0.11cm 3 / g, and the average pore size is 10-11nm.

[0012] A method for preparing the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst as described above comprises the following steps:

[0013] (1) crushing manganese slag, and oxidatively roasting the crushed manganese slag to obtain slag-based Fe2O3;

[0014] (2) adding the obtained slag-based Fe2O3 into a manganese sulfate solution for impregnation and adsorption, filtering, and obtaining filter residue I;

[0015] (3) adding the obtained filter residue I to a NaCl aqueous solution, and adding a persulfate solution, stirring to obtain a suspension;

[0016] (4) The obtained suspension is vigorously stirred and filtered, and the obtained filter residue II is dried to obtain a slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst.

[0017] Furthermore, in step (2), the mass ratio of the slag-based Fe2O3 to the manganese sulfate solution is 1 g:45-50 mL, and the concentration of the manganese sulfate solution is 0.5-1.5 mol / L.

[0018] Furthermore, in step (2), the immersion adsorption is carried out in a shaking table at a rotation speed of 150 to 160 rpm and a temperature of 25 to 26° C. for 11 to 12 hours.

[0019] Furthermore, in step (3), the concentration of the NaCl aqueous solution is 0.01 to 0.07 mol / L, and the concentration of the persulfate solution is 1.25 to 1.75 mol / L.

[0020] Furthermore, in step (4), the vigorous stirring is to place the suspension in a constant temperature water bath at 80 to 90° C. and vigorously stir for 3 to 4 hours.

[0021] Furthermore, in step (4), the drying is to place the filter residue II in a vacuum drying oven and dry it for 11 to 12 hours.

[0022] Furthermore, in step (1), the oxidative roasting is to place the crushed manganese slag in a muffle furnace and oxidatively roast it at 400-700° C. in an air atmosphere for 1-2.5 h.

[0023] Furthermore, in step (1), the manganese slag is crushed to a degree of 300 mesh or more.

[0024] Furthermore, in step (1), the manganese slag is solid waste generated in the process of preparing manganese sulfate using pyrolusite, pyrite and alkylation waste sulfuric acid as main raw materials, and its main components are jarovanadium slag and SiO2.

[0025] An application of the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst as described above in removing ciprofloxacin hydrochloride and Cr(VI) from wastewater.

[0026] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0027] 1. The present invention prepares slag-based Fe2O3 by oxidative roasting of manganese slag, and in-situ grows Na +Doped low-conduction band amorphous MnO2 is used to construct a direct Z-type slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst with oxidation and reduction properties. In this process, manganese ions are anchored on the inner and outer surfaces of slag-based Fe2O3 by impregnation adsorption, and manganese ions are oxidized in a sodium ion solution. Sodium ions can regulate the growth of MnO2 and enter the lattice of MnO2, replacing part of the manganese ions, so that the generated MnO2 is an amorphous structure containing a large number of structural defects, showing a hydrangea-shaped MnO2 in situ growth and anchoring on the slag-based Fe2O3. This hydrangea-shaped shape can greatly increase the specific surface area of ​​slag-based Fe2O3, enhance light absorption and utilization, and expose a large number of active sites, thereby accelerating the efficiency of electron migration and improving photocatalytic activity.

[0028] 2. In the preparation process of the composite material of the present invention, the in-situ grown sodium ion doped amorphous MnO2 has a disordered spatial structure, which makes it more likely to activate H2O2 through non-radical pathways and has higher reaction activity, which can effectively reduce the collision and ineffective consumption of active free radicals. The hydrangea-shaped MnO2 with low crystallinity and low conduction band potential can not only capture and accelerate electron transfer, but also serve as an electron conductive bridge and surface oxygen absorption site, making the separation of photoelectron holes (e-h+) stronger, the electron utilization rate higher, and the photocatalytic activity stronger.

[0029] 3. The present invention uses a slag-based Fe2O3 / MnO2 composite material with high redox performance and reaction activity as a photo-Fenton catalyst for the simultaneous removal of ciprofloxacin hydrochloride and Cr(VI). The degradation rate of ciprofloxacin hydrochloride is more than 81.9%, and the removal rate of Cr(VI) is more than 85.2%. It can effectively reduce the harm of complex pollutants to the environment and has a good application value for the degradation and removal of complex pollutants.

[0030] 4. The preparation method of the composite material of the present invention is an impregnation adsorption-persulfate oxidation method, which is simple to operate, mild reaction conditions, easy to obtain raw materials, low production cost, and suitable for large-scale industrial production. Manganese slag is an industrial waste generated in the process of producing manganese sulfate by acid leaching using pyrolusite and pyrite as the main raw materials. If it is not effectively treated, it will cause serious harm to the ecosystem. The present invention uses manganese slag as the main raw material for oxidative roasting to prepare slag-based Fe2O3 compounds, which can reduce the production cost of raw materials, promote the efficient utilization of manganese slag, and reduce the pollution of industrial waste to the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 XRD patterns of slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts prepared in Example 4.

[0032] Figure 2 These are the SEM images of the slag-based Fe2O3 prepared in Example 4 and the SEM images and EDS images of the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst.

[0033] Figure 3 This is a graph showing the N2 adsorption-desorption curves of the slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts prepared in Example 4.

[0034] Figure 4 UV-visible diffuse reflectance images of slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts prepared in Example 4.

[0035] Figure 5 The photoluminescence spectra of the slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts prepared in Example 4 are shown.

[0036] Figure 6 This is a diagram showing the removal effects of ciprofloxacin hydrochloride and Cr(VI) by the slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts prepared in Example 4. DETAILED DESCRIPTION

[0037] The present invention is further described in detail below by way of examples. These examples are only used to illustrate the present invention and do not limit the protection scope of the present invention.

[0038] Example 1

[0039] Preparation of slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst:

[0040] The manganese slag was crushed to 300 mesh, and a certain amount of the crushed manganese slag was taken and calcined at 400°C for 1h in an air atmosphere to obtain slag-based Fe2O3; 1g of slag-based Fe2O3 was weighed into 50mL of 0.5mol / L manganese sulfate solution, and immersed and adsorbed for 12h in a shaking table at a speed of 150rpm and a constant temperature of 25°C, filtered, and the obtained filter residue I was added to 0.01mol / L sodium chloride solution, and then 1.25mol / L ammonium persulfate was added. After stirring at room temperature for 15min, the obtained suspension was vigorously stirred in a constant temperature water bath at 80°C for 4h, filtered, and the obtained filter residue II was dried in a vacuum drying oven for 12h to obtain a slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst.

[0041] Example 2

[0042] Preparation of slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst:

[0043] The manganese slag was crushed to 500 mesh, and a certain amount of the crushed manganese slag was taken and calcined at 500°C for 1.5h in an air atmosphere to obtain slag-based Fe2O3; 1g of slag-based Fe2O3 was weighed and placed in 50mL of 1.0mol / L manganese sulfate solution, and immersed and adsorbed for 12h in a shaking table at a speed of 150rpm and a constant temperature of 25°C, filtered, and the obtained filter residue I was added to 0.03mol / L sodium chloride solution, and then 1.5mol / L ammonium persulfate was added. After stirring at room temperature for 15min, the obtained suspension was vigorously stirred in a constant temperature water bath at 80°C for 4h, filtered, and the obtained filter residue II was dried in a vacuum drying oven for 12h to obtain a slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst.

[0044] Example 3

[0045] Preparation of slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst:

[0046] The manganese slag was crushed to 700 mesh, and a certain amount of the crushed manganese slag was taken and calcined at 600°C for 2h in an air atmosphere to obtain slag-based Fe2O3; 1g of slag-based Fe2O3 was weighed and placed in 50mL of a 1.5mol / L manganese sulfate solution, and immersed and adsorbed for 12h in a shaking table at a speed of 150rpm and a constant temperature of 25°C, filtered, and the obtained filter residue I was added to a 0.05mol / L sodium chloride solution, and then 1.75mol / L ammonium persulfate was added. After stirring at room temperature for 15min, the obtained suspension was vigorously stirred in a constant temperature water bath at 80°C for 4h, filtered, and the obtained filter residue II was dried in a vacuum drying oven for 12h to obtain a slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst.

[0047] Example 4

[0048] Preparation of slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst:

[0049] The manganese slag was crushed to 900 mesh, and a certain amount of the crushed manganese slag was taken and calcined at 700°C for 2h in an air atmosphere to obtain slag-based Fe2O3; 1g of slag-based Fe2O3 was weighed and placed in 50mL of a 1.5mol / L manganese sulfate solution, and immersed and adsorbed for 12h in a shaking table at a speed of 150rpm and a constant temperature of 25°C, filtered, and the obtained filter residue I was added to a 0.07mol / L sodium chloride solution, and then 1.75mol / L ammonium persulfate was added. After stirring at room temperature for 15min, the obtained suspension was vigorously stirred in a constant temperature water bath at 80°C for 4h, filtered, and the obtained filter residue II was dried in a vacuum drying oven for 12h to obtain a slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst.

[0050] Characterization and Analysis of Slag-based Fe2O3 / MnO2 Composite Photo-Fenton Catalyst

[0051] (I) Chemical composition analysis

[0052] The crystal structures of the slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts prepared in Example 4 of the present invention are as follows: Figure 1 As shown. Figure 1 It can be seen that the slag after oxidative roasting pretreatment is mainly composed of SiO2 and Fe2O3. After amorphous MnO2 is in situ grown by impregnation adsorption and persulfate oxidation, the crystal structure of the composite material does not change significantly compared with the slag-based Fe2O3. No diffraction peak of MnO2 appears in the composite material, indicating that amorphous MnO2 is generated.

[0053] (II) Macromorphology and surface element analysis

[0054] The macroscopic morphology of the slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts prepared in Example 4 of the present invention is as follows: Figure 2 As shown, Figure (a) is the SEM image of slag-based Fe2O3, Figure (b) is the SEM image of slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst, and Figure (c) is the EDS image of slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst. It can be seen from Figures (a) and (b) that after the in-situ growth of MnO2 on the slag-based Fe2O3, MnO2 is anchored on the surface of the slag-based Fe2O3 in a hydrangea-like manner. The formation of this flower-like structure can be simply explained by the formation of S2O8 2- and Mn 2+ Coordinated with deionized water to form MnO6 precursor as the nucleus of MnO2 nanocrystals, during the aging process, the primary particles spontaneously aggregated into fiber units to reduce the surface energy, and these fiber units self-assembled into the hierarchical structure of MnO2 microspheres, and the hierarchical branching growth eventually transformed into a flower-like structure. This special structure can enhance the interaction between metal oxides and carriers, effectively prevent the aggregation of metal oxides, and greatly increase the specific surface area of ​​the composite material. EDS analysis of Figure (c) shows that C, O, Na, Si, Mn and Fe elements are relatively evenly distributed in the slag-based Fe2O3 / MnO2 composite light-Fenton catalyst.

[0055] (III) Specific surface area and pore volume

[0056] The specific surface area and pore size distribution of the slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts prepared in Example 4 were characterized by nitrogen isothermal adsorption-desorption curves. Figure 3 As shown, Figure (a) shows the specific surface area of ​​slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts, and Figure (b) shows the pore size distribution of slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts. Figure 3 It can be seen that the pore structure of slag-based Fe2O3 is mainly composed of mesopores with a pore size of about 11nm, and its specific surface area is only 3.21m 2 / g. The specific surface area of ​​the composite material modified with hydrangea-like amorphous MnO2 increased from 3.21m 2 / g rises to 55.47m 2 / g, which is 17.3 times larger. The larger specific surface area is conducive to the adsorption reaction and provides more active reaction sites for the catalytic reaction.

[0057] (IV) UV-Vis diffuse reflectance spectrum

[0058] The optical properties of the slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts prepared in Example 4 were studied by UV-visible diffuse reflectance. Figure 4 As shown. Figure 4 It can be seen that slag-based Fe2O3 has good light absorption ability in the wavelength range less than 550nm. + After in-situ growth of MnO2 in the solution, the light absorption capacity of the composite material was significantly improved, indicating that MnO2 can effectively improve the visible light absorption capacity of slag-based Fe2O3.

[0059] (V) Electrochemical properties

[0060] The photoluminescence spectrum (PL) was used to characterize the photogenerated electron-hole separation efficiency of the slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts prepared in Example 4. The higher the separation efficiency, the weaker the PL emission peak intensity. The results are as follows: Figure 5 As shown. Figure 5 It can be seen that slag-based Fe2O3 shows a strong emission peak at 460nm, and the recombination rate of photogenerated electrons and holes is relatively fast. When hydrangea-shaped MnO2 is in situ grown on slag-based Fe2O3, slag-based Fe2O3 / MnO2 shows the best separation efficiency of photogenerated electrons and holes, which may be due to the formation of a heterojunction between Fe2O3 and MnO2, which accelerates the transfer of carriers and greatly improves the separation efficiency of photogenerated electrons and holes.

[0061] (VI) Removal effect comparison chart

[0062] The slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts prepared in Example 4 were used in the photo-Fenton reaction to remove ciprofloxacin hydrochloride and Cr(VI). The results are shown in FIG. Figure 6 As shown, Figure (a) and Figure (b) are the removal effects of slag-based Fe2O3 and slag-based Fe2O3 / MnO2 composite photo-Fenton catalysts on Cr(VI) and ciprofloxacin hydrochloride, respectively. Figure 6 It can be seen that when hydrangea-shaped MnO2 was in situ grown on slag-based Fe2O3, the removal efficiency of the composite material for ciprofloxacin hydrochloride and Cr(VI) was significantly improved. Under the reaction conditions (catalyst dosage of 0.5 g / L, H2O2 dosage of 50 μL, reaction time of 1 h, initial pH of 5), the degradation rate of ciprofloxacin hydrochloride was 81.9%, and the Cr(VI) removal rate was 85.2%. When slag-based Fe2O3 was used as a catalyst, the degradation rate of ciprofloxacin hydrochloride was 56.8%, and the Cr(VI) removal rate was 67.9%.

[0063] Application Example 1

[0064] The slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst prepared in Example 1 was applied to the simultaneous removal of ciprofloxacin hydrochloride and Cr(VI) in wastewater. Under the reaction conditions (catalyst dosage of 0.5 g / L, H2O2 dosage of 50 μL, reaction time of 1 h, initial pH of the solution of 5), the degradation rate of ciprofloxacin hydrochloride was 90.4%, and the Cr(VI) removal rate was 91.2%.

[0065] Application Example 2

[0066] The slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst prepared in Example 2 was applied to the simultaneous removal of ciprofloxacin hydrochloride and Cr(VI) in wastewater. Under the reaction conditions (catalyst dosage of 0.5 g / L, H2O2 dosage of 50 μL, reaction time of 1 h, initial pH of 5), the degradation rate of ciprofloxacin hydrochloride was 93.6%, and the Cr(VI) removal rate was 95.3%.

[0067] Application Example 3

[0068] The slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst prepared in Example 3 was applied to the simultaneous removal of ciprofloxacin hydrochloride and Cr(VI) in wastewater. Under the reaction conditions (catalyst dosage of 0.5 g / L, H2O2 dosage of 50 μL, reaction time of 1 h, initial pH of 5), the degradation rate of ciprofloxacin hydrochloride was 98.9% and the Cr(VI) removal rate was 99.2%.

[0069] Application Example 4

[0070] The slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst prepared in Example 4 was applied to the separate removal of ciprofloxacin hydrochloride and Cr(VI) in wastewater. Under the reaction conditions (catalyst dosage of 1 g / L, H2O2 dosage of 150 μL, reaction time of 1 h, initial pH of 5), the degradation rate of ciprofloxacin hydrochloride was 96.6%, and the Cr(VI) removal rate was 97.5%.

Claims

1. A slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst, characterized in that: Slag-based Fe2O3 was prepared by oxidative roasting of manganese slag, and Na2O3 was in situ grown by impregnation adsorption and persulfate oxidation. + Doped low-conduction-band amorphous MnO2 to construct a direct Z-type slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst with oxidation and reduction properties; The specific surface area of ​​the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst is 55-56 m 2 / g, pore volume is 0.10~0.11 cm 3 / g, and the average pore size is 10-11 nm.

2. A method for preparing the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst as claimed in claim 1, characterized in that: The following steps are involved: (1) crushing the manganese slag, and oxidatively roasting the crushed manganese slag to obtain slag-based Fe2O3; (2) adding the obtained slag-based Fe2O3 into a manganese sulfate solution for impregnation and adsorption, filtering, and obtaining filter residue I; (3) Add the obtained filter residue I to a NaCl aqueous solution, add a persulfate solution, and stir to obtain a suspension; (4) The obtained suspension is vigorously stirred and filtered, and the obtained filter residue II is dried to obtain a slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst.

3. The method for preparing the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst according to claim 2, characterized in that: In step (2), the mass ratio of the slag-based Fe2O3 to the manganese sulfate solution is 1 g: 45-50 mL, and the concentration of the manganese sulfate solution is 0.5-1.5 mol / L.

4. The method for preparing the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst according to claim 2, characterized in that: In step (2), the immersion adsorption is carried out in a shaking table at a rotation speed of 150 to 160 rpm and a temperature of 25 to 26° C. for 11 to 12 hours.

5. The method for preparing the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst according to claim 2, characterized in that: In step (3), the concentration of the NaCl aqueous solution is 0.01 to 0.07 mol / L, and the concentration of the persulfate solution is 1.25 to 1.75 mol / L.

6. The method for preparing the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst according to claim 2, characterized in that: In step (4), the vigorous stirring is to place the suspension in a constant temperature water bath at 80 to 90° C. and vigorously stir for 3 to 4 hours.

7. The method for preparing the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst according to claim 2, characterized in that: In step (4), the drying step is to place the filter residue II in a vacuum drying oven and dry it for 11 to 12 hours.

8. The method for preparing the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst according to claim 2, characterized in that: In step (1), the oxidative roasting is to place the crushed manganese slag in a muffle furnace and oxidatively roast it at 400-700° C. in an air atmosphere for 1-2.5 h.

9. Use of the slag-based Fe2O3 / MnO2 composite photo-Fenton catalyst as claimed in claim 1 in the simultaneous removal of ciprofloxacin hydrochloride and Cr(VI) in wastewater.

Citation Information

Patent Citations

  • Preparation method of heterogeneous Fenton catalyst taking protein earth as carrier

    CN106799235A