A kind of cellulose triacetate film and preparation method thereof

By optimizing the formulation of cellulose triacetate films, combining cellulose acylate, sugar esters compounds and cellulose acetate-propanoate and other materials, the problems of poor moisture permeability and low durability of films in the prior art are solved. It achieves higher weather resistance and dimensional stability, extending the service life of the product.

CN116102793BActive Publication Date: 2024-11-05LUCKY OPTOELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211641507.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-20
Publication Date
2024-11-05
Estimated Expiration
2042-12-20

AI Technical Summary

Technical Problem

The existing cellulose acetate films have poor moisture permeability, low durability, poor dimensional stability and poor compatibility of plasticizers with cellulose ester in liquid crystal display devices, resulting in the decline in performance of the product in harsh environments and service life. short.

Method used

By optimizing the formulation of cellulose triacetate films, increasing the acetyl substitution and polymerization degree of cellulose acylate esters, combining the mass ratio of sugar ester compounds and maleic anhydride modified ethylene-vinyl acetate, using acetic acid-propylene acetate Cellulose acid is used as a toughening agent, and an appropriate amount of ultraviolet absorber and matting agent is added to improve the tensile and fracture performance, transparency and water-blocking properties of the film. At the same time, the ratio of plasticizer to ultraviolet absorber is adjusted to improve the weather resistance of the film. and dimensional stability.

Benefits of technology

It improves the transparency, tensile strength and water-blocking properties of the triacetate ester film, extends the service life of the product, enhances the tolerance to ultraviolet rays, temperature and humidity, and reduces the exudation and precipitation of plasticizers. Improves the mechanical properties and appearance quality of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004007700080000241
    Figure BDA0004007700080000241
  • Figure BDA0004007700080000251
    Figure BDA0004007700080000251
  • Figure BDA0004007700080000261
    Figure BDA0004007700080000261
Patent Text Reader

Abstract

The invention discloses a cellulose triacetate film and a preparation method thereof. The cellulose triacetate film has excellent water-blocking, durability and dimensional stability, has good compatibility between a plasticizer and a toughening agent and the cellulose triacetate, can greatly reduce precipitation, improves the appearance quality of the product, and has more excellent optical properties. In addition, the film has certain weather resistance and moisture permeability, good mechanical properties and a prolonged service life. The preparation method of the invention does not need to add a coating process, and is simpler and more economical in terms of process and energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of TAC films, with the classification number being C08J7 / 04, and in particular to a cellulose triacetate film and a preparation method thereof. Background Art

[0002] Polarizer is an essential component of liquid crystal display, which is composed of polarizing film and protective film. Polarizing film is made of polyvinyl alcohol film impregnated with iodide solution and then stretched longitudinally, which has polarizing effect on light. After stretching, the mechanical strength of polarizing film is very poor, and the oriented iodine molecules are easily affected by external moisture and change their orientation degree, which affects its polarization effect. Cellulose triacetate film is widely used as protective film of polarizer due to its excellent physical and optical properties. It is pasted on both sides of polarizing film, which not only improves its physical and mechanical properties, but also isolates it from the influence of external water vapor to a certain extent.

[0003] Cellulose triacetate film usually adds one or more of triphenyl phosphate, 2-biphenyl diphenyl phosphate, 4-biphenyloxy diphenyl phosphate, tris(xylenol) phosphate, and resorcinol tetraphenyl diphosphate as plasticizers to improve its mechanical properties. However, in recent years, liquid crystal display devices are developing towards thinning, and polarizer protective films are also being thinned accordingly. There are three problems with phosphate ester thinned cellulose triacetate films: First, the amount of phosphate ester plasticizer added is large, and precipitation is serious, which greatly affects the production system and product appearance quality; second, the product durability is poor, which is mainly reflected in the degradation of the auxiliary agent after moisture permeation, which accelerates the degradation of the triacetate cellulose film, thereby affecting the service life of the liquid crystal display device; third, the product dimensional stability is poor, and the polarization degree of the polarizer produced is reduced. With the widespread use of modern display devices outdoors, in order to cope with harsh environments such as high and low temperatures, humidity and heat, and ultraviolet radiation, liquid crystal display devices and their constituent materials are required to be more excellent in weather resistance, and more excellent in medium-sized displays such as flat panels, vehicles, and computers. Generally speaking, the moisture permeability of cellulose triacetate film can be reduced and weather resistance can be improved by increasing the amount of plasticizer used. However, conventional plasticizers have poor compatibility with cellulose triacetate. When the amount is increased, it is easy to seep out of the film surface under hot and humid conditions, which also aggravates the degradation of the product and affects the product appearance and service life.

[0004] As a method to solve the above problem, Chinese Patent CN105988155A, Japanese Patent Publication No. 2006-083225 and Japanese Patent Publication No. 2011-93133 adopt a coating method to apply a hard coating on at least one side of a triacetyl cellulose film to improve the moisture permeability of the film. However, the above method requires secondary processing or adding a coating process to the original equipment, but either method will greatly increase the production cost and operation complexity of the film. Summary of the invention

[0005] In view of the above problems existing in the prior art, a triacetyl cellulose film is provided. The specific technical scheme is as follows: a triacetyl cellulose film, whose raw materials include, by weight: 80-100 parts of acylated cellulose, 5-20 parts of plasticizer, 1-10 parts of toughening agent, 100-300 parts of solvent, 10-50 parts of alcohol with 1-4 carbon atoms, 0.1-3 parts of ultraviolet absorber, and 0.1-2 parts of matting agent.

[0006] Further preferably, the raw materials of the cellulose triacetate film include, by weight: 90-100 parts of cellulose acylate, 7-20 parts of plasticizer, 3-10 parts of toughening agent, 100-200 parts of solvent, 20-40 parts of alcohol having 1-4 carbon atoms, 0.8-2.5 parts of ultraviolet absorber, and 0.1-0.5 parts of matting agent.

[0007] Further preferably, the raw materials of the cellulose triacetate film include, by weight: 100 parts of cellulose acylate, 7-15 parts of plasticizer, 3-6 parts of toughening agent, 150-200 parts of solvent, 20-30 parts of alcohol having 1-4 carbon atoms, 0.8-1.5 parts of ultraviolet absorber, and 0.3-0.5 parts of matting agent.

[0008] Further preferably, the raw materials of the cellulose triacetate film include, by weight: 100 parts of cellulose acylate, 10 parts of plasticizer, 5 parts of toughening agent, 177 parts of solvent, 23 parts of alcohol having 1-4 carbon atoms, 1.0 part of ultraviolet absorber, and 0.5 part of matting agent.

[0009] More preferably, the solvent is at least one of dichloromethane, chloroform, acetone, butanone, ethyl acetate, methyl acetate, propyl acetate, and butyl acetate; the alcohol having 1 to 4 carbon atoms is at least one of methanol, ethanol, butanol, propanol, isopropanol, and isobutanol; the ultraviolet absorber is 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2-hydroxy-5-methyl At least one of 2,2'-dihydroxy-4,4'-dimethoxybenzophenone and 2,2,4,4-tetrahydroxybenzophenone; and the matting agent is at least one of silicon dioxide, a silicon dioxide derivative, titanium dioxide and zirconium oxide.

[0010] More preferably, the solvent is dichloromethane, the alcohol having an atomic number of 1-4 is methanol, the ultraviolet absorber is 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl), and the matting agent is silicon dioxide.

[0011] More preferably, the particle size of the silicon dioxide is 0.01 μm-1 μm.

[0012] More preferably, the particle size of the silicon dioxide is 0.06 μm.

[0013] Preferably, the cellulose acylate has an acetyl substitution degree of 60-70 and a polymerization degree of 260-350.

[0014] The applicant has found that when the acetyl substitution degree of cellulose acylate is 60-70 and the polymerization degree is 260-350, the compatibility of cellulose acylate with plasticizers and toughening agents is enhanced, so that the obtained cellulose triacetate film has good light transmission performance and mechanical strength.

[0015] More preferably, the cellulose acylate has an acetyl substitution degree of 60.4-61 and a polymerization degree of 320-350.

[0016] More preferably, the cellulose acylate has an acetyl substitution degree of 60.4 and a polymerization degree of 350.

[0017] Preferably, the plasticizer is a sugar ester compound and maleic anhydride modified ethylene-vinyl acetate, and the weight ratio of the two is (2-12): (3-8).

[0018] More preferably, the plasticizer is a sugar ester compound and maleic anhydride modified ethylene vinyl acetate, and the weight ratio of the two is (2-8): (5-8).

[0019] The applicant has found that when the plasticizer ester compound maleic anhydride modifies ethylene-vinyl acetate and the weight ratio of the two is (2-8): (5-8), the tensile fracture performance of the film can be improved. It is speculated that: the plasticizer ester compound and maleic anhydride modified ethylene-vinyl acetate at this time have excellent affinity and compatibility with cellulose triacetate, which makes the intermolecular force lower, the dispersion state between the systems more uniform, and the various mixtures have a high degree of isotropy, which suppresses the anisotropy in cellulose triacetate. In addition, the cellulose triacetate film is easier to peel off from the cast stainless steel belt, reducing the peeling mark defect and improving the product appearance quality.

[0020] Further preferably, the plasticizer is a sugar ester compound and maleic anhydride modified ethylene-vinyl acetate in a weight ratio of 3:7.

[0021] Preferably, the relative molecular weight of the sugar ester compound is 300-1500.

[0022] More preferably, the relative molecular weight of the sugar ester compound is 300-500.

[0023] Further preferably, the relative molecular weight of the sugar ester compound is 466.

[0024] Further preferably, the sugar ester compound is sucrose benzoate.

[0025] Preferably, the maleic anhydride modified ethylene vinyl acetate has a viscosity of 1700-3000 mPa.s.

[0026] The applicant has found that when the viscosity of maleic anhydride modified ethylene-vinyl acetate is between 1700 and 3000 mPa.s, it is not easy to cause exudation, and the transparency and tensile strength of the cellulose triacetate film are improved. Under the joint action of the toughening agent and the matting agent, it also has certain water-blocking and moisture-permeable properties, which can prevent external moisture from affecting the polarizing film, while maintaining a certain moisture permeability, so that the glue after the polarizing film is compounded can be effectively volatilized.

[0027] Further preferably, the maleic anhydride modified ethylene vinyl acetate has a viscosity of 2000-2500 mPa.s.

[0028] Further preferably, the viscosity of the maleic anhydride modified ethylene vinyl acetate is 2200 mPa.s.

[0029] Preferably, the toughening agent is cellulose acetate-propionate, the acetyl molar percentage of which is 7.5%-9.0%, the propionyl molar percentage of which is 39%-47%, and the relative molecular weight of which is 450-550.

[0030] The applicant found that when the molar percentage of acetyl in the toughening agent is 7.5%-9.0% and the molar percentage of propionyl is 39%-47%, the dimensional stability and durability of the film are improved and the service life of the product is extended. It is speculated that: with the increase of the molar percentage of acetyl, the melting point and tensile strength of cellulose acetate-propionate are increased, and the durability and dimensional stability are enhanced, but its compatibility with the plasticizer and the flexibility of the film are reduced within a certain range. The increase in the molar percentage of propionyl reduces the density of CAP and improves its compatibility with the plasticizer, but it will cause the durability and stability of the film to decrease. Therefore, when the molar percentage of acetyl in the toughening agent is 7.5%-9.0% and the molar percentage of propionyl is 39%-47%, the dimensional stability and durability of the film are improved, and the service life of the product is extended. Therefore, the present application sets the molar percentage of acetyl in the toughening agent to 7.5%-9.0% and the molar percentage of propionyl to 39%-47%.

[0031] Further preferably, the toughening agent is cellulose acetate-propionate, the acetyl molar percentage of which is 8.0%, the propionyl molar percentage of which is 42%, and the relative molecular weight of which is 500.

[0032] Preferably, the mass ratio of the plasticizer to the ultraviolet absorber is (7-20): (0.1-1.5).

[0033] Further preferably, the mass ratio of the plasticizer to the ultraviolet absorber is (7-15): (0.5-1.5). The applicant has found that when the mass ratio of the plasticizer to the ultraviolet absorber is (7-15): (0.5-1.5), not only the weather resistance of the triacetylcellulose film is enhanced, but also the effects of ultraviolet rays, temperature, humidity, and time can be alleviated to a large extent, and the problems of plasticizer and ultraviolet absorber seepage, atomization, and solid precipitation on the film surface can be solved, ensuring that the product appearance, optical properties, mechanical properties, and ultraviolet resistance are more excellent and stable.

[0034] Further preferably, the mass ratio of the plasticizer to the ultraviolet absorber is 10:1.

[0035] Preferably, the mass ratio of the cellulose acylate to the plasticizer is 100:(7-20).

[0036] The applicant has found that when the mass ratio of cellulose triacetate and the plasticizer mixture is 100:(7-20), the plasticizer is not easy to deposit. When the mass ratio is below 100:7, the anisotropy of the dispersed state of cellulose ester disappears and the isotropy becomes larger, thereby weakening the intermolecular force of the cellulose ester resin. Therefore, when the mass ratio of cellulose triacetate and the plasticizer mixture is 100:(7-20), not only the transparency and tensile fracture performance of the cellulose triacetate film are improved, but also the cellulose triacetate film can still have excellent bonding performance after being saponified with alkali solution, and is easier to be bonded with the polarizing film, thereby improving the yield rate of the polarizing film.

[0037] More preferably, the mass ratio of the cellulose acylate to the plasticizer is 100:(7-15).

[0038] Further preferably, the mass ratio of the cellulose acylate to the plasticizer is 100:10.

[0039] Preferably, the thickness of the cellulose triacetate film is 30-70 μm.

[0040] More preferably, the cellulose triacetate film has a thickness of 50-70 μm.

[0041] More preferably, the thickness of the cellulose triacetate film is 60 μm.

[0042] The second aspect of the present invention provides a method for preparing a cellulose triacetate film, the specific steps of which are as follows:

[0043] S1: Add alcohol methanol with carbon number 1-4 into cellulose ester dissolving kettle by weight, add cellulose acylate at a stirring speed of 500-800rpm / min, stir for 1-2min, then add solvent dichloromethane and methanol, continue stirring for 5-6min, and then add cotton glue solution into the feeding pump.

[0044] S2: Filter the cotton glue solution;

[0045] After the cotton glue solution in the feed pump is filtered by the first filter and the second filter, it is added to the defoaming storage for storage and standby use.

[0046] S3: mixing the plasticizer with the filtered cotton glue solution to prepare a first dispersion;

[0047] Sugar ester compounds and maleic anhydride modified ethylene-vinyl acetate are added to a plasticizer mixing kettle by weight, and dispersed and dissolved by the combined action of ultrasonic cavitation effect and mechanical stirring. After 10 minutes to 30 minutes, the mixture is added to a third filter for filtration at 40 to 50° C., with a filtration accuracy of less than 7 μm. Afterwards, the mixture is added to a first static mixer and mixed with the cotton glue solution filtered in step S2, and then added to a medium storage to obtain a first dispersion.

[0048] S4: mixing the toughening agent with the first dispersion to obtain a second dispersion;

[0049] Dissolve the toughening agent in a CAP cotton glue mixing kettle with methanol and dichloromethane according to weight, filter through a fourth filter and then transfer to a second static mixer, add the filtrate to the intermediate storage to obtain a second dispersion;

[0050] S5: adding a matting agent and a UV absorber into the second dispersion to prepare a semi-finished product;

[0051] First, the matting agent is mixed in a matting agent mixing kettle according to weight parts, filtered through a fifth filter and set aside, then the ultraviolet absorber is added to the ultraviolet absorber mixing kettle, stirred for 10-30 minutes, the obtained dispersion is added to the fifth filter and filtered, and then mixed with the matting agent to obtain an ultraviolet absorber-matting agent mixed liquid, and then the mixed liquid is mixed with the second dispersion in the intermediate storage in a third static mixer to obtain a semi-finished product.

[0052] S6: The semi-finished product is cast and stretched by a casting machine, and then pre-dried, peeled, dried again, and rolled up in a drying oven to obtain a cellulose triacetate film.

[0053] Further preferably, the mass ratio of dichloromethane to methanol in step S1 is 87:13, and the mass ratio of dichloromethane to methanol in step S4 is 90:10. The above technical solution has the following advantages or beneficial effects:

[0054] (1) The present invention improves the tensile fracture properties of the film by limiting the mass ratio of the plasticizer sugar ester compound and the maleic anhydride modified ethylene-vinyl acetate, making the cellulose triacetate film easier to peel off from the cast stainless steel belt, reducing the peeling mark defect, and improving the product appearance quality.

[0055] (2) The present invention improves the transparency and tensile strength of the cellulose triacetate film by limiting the viscosity of maleic anhydride-modified ethylene-vinyl acetate. Under the joint action of the toughening agent and the matting agent, the film also has certain water-blocking and moisture-permeability properties, which can prevent external moisture from affecting the polarizing film while maintaining a certain moisture permeability, so that the glue after the polarizing film is compounded can be effectively volatilized.

[0056] (3) The present invention improves the dimensional stability and durability of the film and prolongs the service life of the product by adding a toughening agent with a certain molar percentage of acetyl and propionyl.

[0057] (4) The present invention limits the mass ratio of cellulose triacetate to plasticizer, which is beneficial to improving the weather resistance of cellulose triacetate film, and has excellent resistance to ultraviolet rays, cold, and moisture and heat. Under the joint action of the toughening agent, the dimensional stability of the cellulose triacetate film is improved, and its transverse and longitudinal shrinkage rates are kept consistent with the shrinkage of PVA, thereby improving the durability of the polarizer and extending the service life.

[0058] (5) The preparation method of the present invention does not require the addition of a coating process, and is simpler and more economical in terms of process and energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] The embodiments of the present invention will be described more fully with reference to the attached drawings, which are provided for illustration and description only and are not intended to limit the scope of the present invention.

[0060] Figure 1 It is a schematic diagram of the specific structure of the dissolution and filtration equipment.

[0061] Figure 2 It is a schematic diagram of the equipment structure for preparing semi-finished products into finished products.

[0062] Figure 1 The serial numbers are as follows: 1-cellulose ester dissolving kettle; 2-feeding pump; 3-first filter; 4-second filter; 5-defoaming intermediate storage; 6-first static mixer; 7-intermediate storage; 8-second static mixer; 9-intermediate storage; 10-third static mixer; 11-plasticizer mixing kettle; 12-third filter; 13-CAP cotton glue mixing kettle; 14-fourth filter; 15-matting agent mixing kettle; 16-fifth filter; 17-ultraviolet absorber mixing kettle; 18-sixth filter.

[0063] Figure 2 The serial numbers are as follows: 19-casting machine; 20-stretching machine; 21-drying box; 22-winding. DETAILED DESCRIPTION

[0064] The present invention is further described below in conjunction with specific implementation cases, but the present invention is not limited thereto.

[0065] Example 1

[0066] A cellulose triacetate film, characterized in that, in parts by weight, its raw materials include: 100 parts of cellulose acylate, 15 parts of a plasticizer, 8 parts of a toughening agent, 200 parts of a solvent, 22 parts of an alcohol having 1 to 4 carbon atoms, 0.5 parts of an ultraviolet absorber, and 0.15 parts of a matting agent.

[0067] The cellulose acylate is cellulose triacetate, with an acetyl substitution degree of 60.4 and a polymerization degree of 350. It is purchased from Daicel Japan, and the model number is LT-1054.

[0068] The plasticizers are sugar ester compounds and maleic anhydride modified ethylene-vinyl acetate, and the weight ratio of the two is 8:7.

[0069] The mass ratio of the cellulose acylate to the plasticizer is 100:15.

[0070] The sugar ester compound is sucrose benzoate, with a relative molecular weight of 466, purchased from Zhejiang Hetang Technology, model number TZ-3.

[0071] The maleic anhydride modified ethylene-vinyl acetate has a viscosity of 1700 mPa.s and is purchased from DIC Corporation with a model number of W48S.

[0072] The toughening agent is cellulose acetate-propionate, with an acetyl molar percentage of 8.0%, a propionyl molar percentage of 42%, a relative molecular weight of 500, purchased from Eastman, USA, model 482A.

[0073] The ultraviolet absorber is 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, purchased from Tianjin Lianlong, model number UV326.

[0074] The mass ratio of the plasticizer to the ultraviolet absorber is 15:0.5.

[0075] The matting agent is silicon dioxide with a particle size of 0.06 μm, purchased from Evonik of Germany, model number R972.

[0076] The solvent is dichloromethane, and the alcohol having 1 to 4 carbon atoms is methanol.

[0077] The second aspect of this embodiment provides a method for preparing a cellulose triacetate film, and the specific steps are as follows:

[0078] S1: Add alcohol with 1-4 carbon atoms by weight into a cellulose ester dissolving kettle, add cellulose acylate at a stirring speed of 700 rpm / min, stir for 2 minutes, then add dichloromethane and methanol, continue stirring for 5 minutes, and then add the cotton glue solution into the feed pump.

[0079] S2: Filter the cotton glue solution;

[0080] After the cotton glue solution in the feed pump is filtered by the first filter and the second filter, it is added to the defoaming storage for storage and standby use.

[0081] S3: mixing the plasticizer with the filtered cotton glue solution to prepare a first dispersion;

[0082] Sugar ester compounds and maleic anhydride modified ethylene-vinyl acetate are added to the plasticizer mixing kettle according to weight, and dispersed and dissolved by the combined action of ultrasonic cavitation effect and mechanical stirring. After 20 minutes, they are added to the third filter for filtration at 45°C, and the filtration accuracy is <7μm. After that, they are added to the first static mixer and mixed with the cotton glue solution filtered in step S2, and then added to the intermediate storage to obtain the first dispersion.

[0083] S4: mixing the toughening agent with the first dispersion to obtain a second dispersion;

[0084] Dissolve the toughening agent in a CAP cotton glue mixing kettle with methanol and dichloromethane according to weight, filter through a fourth filter and then transfer to a second static mixer, add the filtrate to the intermediate storage to obtain a second dispersion;

[0085] S5: adding a matting agent and a UV absorber into the second dispersion to prepare a semi-finished product;

[0086] First, the matting agent is mixed in a matting agent mixing kettle according to weight parts, filtered through a fifth filter and set aside, then the ultraviolet absorber is added to the ultraviolet absorber mixing kettle, stirred for 20 minutes, the obtained dispersion is added to the fifth filter and filtered, and then mixed with the matting agent to obtain an ultraviolet absorber-matting agent mixed liquid, and then the mixed liquid is mixed with the second dispersion in the intermediate storage in a third static mixer to obtain a semi-finished product.

[0087] S6: The semi-finished product is cast and stretched by a casting machine, and then pre-dried, peeled, dried again, and rolled up in a drying oven to obtain a cellulose triacetate film.

[0088] Further preferably, the mass ratio of dichloromethane to methanol in step S1 is 87:13, and the mass ratio of dichloromethane to methanol in step S4 is 90:10.

[0089] The thickness of the cellulose triacetate film is 70 μm.

[0090] Example 2

[0091] A cellulose triacetate film, characterized in that, by weight, its raw materials include: 100 parts of cellulose acylate, 10 parts of plasticizer, 7 parts of toughening agent, 177 parts of solvent, 23 parts of alcohol with 1-4 carbon atoms, 1.0 part of ultraviolet absorber, and 0.2 part of matting agent.

[0092] The cellulose acylate is cellulose triacetate, with an acetyl substitution degree of 60.7 and a polymerization degree of 260. It was purchased from Sichuan Pushi, model number H11872.

[0093] The plasticizer is a sugar ester compound and maleic anhydride modified ethylene-vinyl acetate, and the weight ratio of the two is 5:5.

[0094] The mass ratio of the cellulose acylate to the plasticizer is 100:10.

[0095] The sugar ester compound has a relative molecular weight of 300 and is purchased from Zhejiang Hetang Technology with a model number of TZ-2.

[0096] The maleic anhydride modified ethylene-vinyl acetate has a viscosity of 3500 mPa.s and is purchased from DIC Corporation with a model number of 6540A.

[0097] The toughening agent is cellulose acetate-propionate, with an acetyl molar percentage of 9.0%, a propionyl molar percentage of 39%, a relative molecular weight of 480, purchased from Eastman, USA, model 380A.

[0098] The ultraviolet absorber is 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl), purchased from Tianjin Lianlong, model number UV928.

[0099] The mass ratio of the plasticizer to the ultraviolet absorber is 10:1.

[0100] The matting agent is silicon dioxide with a particle size of 0.06 μm, purchased from Evonik of Germany, model number R972.

[0101] The solvent is dichloromethane, and the alcohol having 1 to 4 carbon atoms is methanol.

[0102] The thickness of the cellulose triacetate film is 30 μm.

[0103] The rest is the same as in Example 1.

[0104] Example 3

[0105] A cellulose triacetate film, characterized in that, by weight, its raw materials include: 100 parts of cellulose acylate, 10 parts of plasticizer, 5 parts of toughening agent, 177 parts of solvent, 23 parts of alcohol with 1-4 carbon atoms, 1.0 part of ultraviolet absorber, and 0.15 part of matting agent.

[0106] The cellulose acylate is cellulose triacetate, with an acetyl substitution degree of 60.4 and a polymerization degree of 350. It is purchased from Daicel Japan, and the model number is LT-1054.

[0107] The plasticizers are sugar ester compounds and maleic anhydride modified ethylene-vinyl acetate, and the weight ratio of the two is 3:7.

[0108] The mass ratio of the cellulose acylate to the plasticizer is 100:10.

[0109] The sugar ester compound is sucrose benzoate, with a relative molecular weight of 466, purchased from Zhejiang Hetang Technology, model number TZ-3.

[0110] The maleic anhydride modified ethylene-vinyl acetate has a viscosity of 2200 mPa.s and is purchased from DIC Corporation with a model number of 6250.

[0111] The toughening agent is cellulose acetate-propionate, with an acetyl molar percentage of 8.0%, a propionyl molar percentage of 42%, a relative molecular weight of 500, purchased from Eastman, USA, model 482A.

[0112] The ultraviolet absorber is 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl), purchased from Tianjin Lianlong, model number UV928.

[0113] The mass ratio of the plasticizer to the ultraviolet absorber is 10:1.

[0114] The matting agent is silicon dioxide with a particle size of 0.06 μm, purchased from Evonik of Germany, model number R972.

[0115] The solvent is dichloromethane, and the alcohol having 1 to 4 carbon atoms is methanol.

[0116] The thickness of the cellulose triacetate film is 60 μm.

[0117] The rest is the same as in Example 1.

[0118] Example 4

[0119] A cellulose triacetate film, characterized in that, in parts by weight, its raw materials include: 80 parts of cellulose acylate, 10 parts of a plasticizer, 1 part of a toughening agent, 100 parts of a solvent, 10 parts of an alcohol having 1 to 4 carbon atoms, 0.1 parts of an ultraviolet absorber, and 2.0 parts of a matting agent.

[0120] The cellulose acylate is cellulose triacetate, with an acetyl substitution degree of 60.4 and a polymerization degree of 300. It was purchased from Daicel Japan, model number LT-100.

[0121] The plasticizer is a sugar ester compound and maleic anhydride modified ethylene-vinyl acetate, and the weight ratio of the two is 5:5.

[0122] The mass ratio of the cellulose acylate to the plasticizer is 80:10.

[0123] The sugar ester compound has a relative molecular weight of 300 and is purchased from Zhejiang Hetang Technology with a model number of TZ-2.

[0124] The maleic anhydride modified ethylene-vinyl acetate has a viscosity of 3000 mPa.s and is purchased from DIC Corporation with a model number of 6540A.

[0125] The toughening agent is cellulose acetate-propionate, with an acetyl molar percentage of 8.0%, a propionyl molar percentage of 42%, a relative molecular weight of 500, purchased from Eastman, USA, model 482A.

[0126] The ultraviolet absorber is 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, purchased from Tianjin Lianlong, model number UV326.

[0127] The mass ratio of the plasticizer to the ultraviolet absorber is 10:0.1.

[0128] The matting agent is silicon dioxide with a particle size of 0.06 μm, purchased from Evonik of Germany, model number R972.

[0129] The solvent is dichloromethane, and the alcohol having 1 to 4 carbon atoms is methanol.

[0130] The thickness of the cellulose triacetate film is 40 μm.

[0131] The rest is the same as in Example 1.

[0132] Example 5

[0133] A cellulose triacetate film, characterized in that, in parts by weight, its raw materials include: 90 parts of cellulose acylate, 8 parts of plasticizer, 10 parts of toughening agent, 300 parts of solvent, 50 parts of alcohol with 1-4 carbon atoms, 3.0 parts of ultraviolet absorber, and 0.1 part of matting agent.

[0134] The cellulose acylate is cellulose triacetate, with an acetyl substitution degree of 60.7 and a polymerization degree of 260, purchased from Sichuan Pushi, model number H11872.

[0135] The plasticizers are sugar ester compounds and maleic anhydride modified ethylene-vinyl acetate, and the weight ratio of the two is 3:5.

[0136] The mass ratio of the cellulose acylate to the plasticizer is 90:8.

[0137] The sugar ester compound has a relative molecular weight of 1500 and is purchased from Zhejiang Hetang Technology with a model number of TZ-1.

[0138] The maleic anhydride modified ethylene-vinyl acetate has a viscosity of 1700 mPa.s and is purchased from DIC Corporation with a model number of W48S.

[0139] The toughening agent is cellulose acetate-propionate, with an acetyl molar percentage of 9.0%, a propionyl molar percentage of 39%, a relative molecular weight of 480, purchased from Eastman, USA, model 380A.

[0140] The ultraviolet absorber is 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, purchased from Tianjin Lianlong, model number UV329.

[0141] The mass ratio of the plasticizer to the ultraviolet absorber is 8:3.

[0142] The matting agent is silicon dioxide with a particle size of 0.06 μm, purchased from Evonik of Germany, model number R972.

[0143] The solvent is dichloromethane, and the alcohol having 1 to 4 carbon atoms is methanol.

[0144] The thickness of the cellulose triacetate film is 60 μm.

[0145] The rest is the same as in Example 1.

[0146] Comparative Example 1

[0147] A cellulose triacetate film, characterized in that, by weight, its raw materials include: 100 parts of cellulose acylate, 10 parts of plasticizer, 177 parts of solvent, 22 parts of alcohol with 1-4 carbon atoms, 1.0 part of ultraviolet absorber, and 0.15 part of matting agent.

[0148] The cellulose acylate is cellulose triacetate, with an acetyl substitution degree of 60.4 and a polymerization degree of 350, purchased from Daicel Japan, with a model number of LT-1054.

[0149] The plasticizers are 4-biphenyloxy diphenyl phosphate and triphenyl phosphate, and the weight ratio of the two is 7:3.

[0150] The mass ratio of the cellulose acylate to the plasticizer is 100:10.

[0151] The 4-biphenyloxy diphenyl phosphate was purchased from Hubei Xinkang Pharmaceutical Chemical Co., Ltd. with a CAS number of 17269-99-7.

[0152] The triphenyl phosphate was purchased from LANXESS, Germany, with the model number being UN3077.

[0153] The ultraviolet absorber is 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl), purchased from Tianjin Lianlong, model number UV928.

[0154] The mass ratio of the plasticizer to the ultraviolet absorber is 10:1.

[0155] The matting agent is silicon dioxide with a particle size of 0.06 μm, purchased from Evonik of Germany, model number R972.

[0156] The solvent is dichloromethane, and the alcohol having 1 to 4 carbon atoms is methanol.

[0157] The second aspect of this embodiment provides a method for preparing a cellulose triacetate film, and the specific steps are as follows:

[0158] S1: Add alcohol with 1-4 carbon atoms by weight into a cellulose ester dissolving kettle, add cellulose acylate at a stirring speed of 700 rpm / min, stir for 2 minutes, then add dichloromethane and methanol, continue stirring for 5 minutes, and then add the cotton glue solution into the feed pump.

[0159] S2: Filter the cotton glue solution;

[0160] After the cotton glue solution in the feed pump is filtered by the first filter and the second filter, it is added to the defoaming storage for storage and standby use.

[0161] S3: mixing the plasticizer with the filtered cotton glue solution to prepare a first dispersion;

[0162] 4-Biphenyloxy diphenyl phosphate and triphenyl phosphate are added to the plasticizer mixing kettle by weight, and dispersed and dissolved by the combined action of ultrasonic cavitation effect and mechanical stirring. After 20 minutes, they are added to the third filter for filtration at 45°C, and the filtration accuracy is less than 7μm. After that, they are added to the first static mixer and mixed with the cotton glue solution filtered in step S2, and then added to the intermediate storage to obtain the first dispersion.

[0163] S4: adding a matting agent and a UV absorber into the first dispersion to prepare a semi-finished product;

[0164] First, the matting agent is mixed in a matting agent mixing kettle according to weight parts, filtered through a fifth filter and set aside, then the ultraviolet absorber is added to the ultraviolet absorber mixing kettle, stirred for 20 minutes, the obtained dispersion is added to the fifth filter and filtered, and then mixed with the matting agent to obtain an ultraviolet absorber-matting agent mixed liquid, and then the mixed liquid is mixed with the first dispersion in the intermediate storage in a third static mixer to obtain a semi-finished product.

[0165] S5: The semi-finished product is cast and stretched by a casting machine, and then pre-dried, peeled, dried again, and rolled up in a drying oven to obtain a cellulose triacetate film.

[0166] Further preferably, the mass ratio between dichloromethane and methanol in step S1 is 89:11.

[0167] The thickness of the cellulose triacetate film is 60 μm.

[0168] Comparative Example 2

[0169] A cellulose triacetate film, characterized in that, in parts by weight, its raw materials include: 100 parts of cellulose acylate, 10 parts of a plasticizer, 200 parts of a solvent, 22 parts of an alcohol having 1 to 4 carbon atoms, 0.5 parts of an ultraviolet absorber, and 0.1 parts of a matting agent.

[0170] The cellulose acylate is cellulose triacetate, with an acetyl substitution degree of 60.4 and a polymerization degree of 300. It was purchased from Daicel Japan, model number LT-100.

[0171] The plasticizers are 4-biphenyloxy diphenyl phosphate and triphenyl phosphate, and the weight ratio of the two is 5:5.

[0172] The mass ratio of the cellulose acylate to the plasticizer is 100:10.

[0173] The 4-biphenyloxy diphenyl phosphate was purchased from Hubei Xinkang Pharmaceutical Chemical Co., Ltd. with a CAS number of 17269-99-7.

[0174] The triphenyl phosphate was purchased from LANXESS, Germany, with the model number being UN3077.

[0175] The ultraviolet absorber is 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, purchased from Tianjin Lianlong, model number UV326.

[0176] The mass ratio of the plasticizer to the ultraviolet absorber is 10:0.5.

[0177] The matting agent is silicon dioxide with a particle size of 0.06 μm, purchased from Evonik of Germany, model number R972.

[0178] The solvent is dichloromethane, and the alcohol having 1 to 4 carbon atoms is methanol.

[0179] The second aspect of this embodiment provides a method for preparing a cellulose triacetate film, and the specific steps are as follows:

[0180] S1: Add alcohol with 1-4 carbon atoms by weight into a cellulose ester dissolving kettle, add cellulose acylate at a stirring speed of 700 rpm / min, stir for 2 minutes, then add dichloromethane and methanol, continue stirring for 5 minutes, and then add the cotton glue solution into the feed pump.

[0181] S2: Filter the cotton glue solution;

[0182] After the cotton glue solution in the feed pump is filtered by the first filter and the second filter, it is added to the defoaming storage for storage and standby use.

[0183] S3: mixing the plasticizer with the filtered cotton glue solution to prepare a first dispersion;

[0184] 4-Biphenyloxy diphenyl phosphate and triphenyl phosphate are added to the plasticizer mixing kettle by weight, and dispersed and dissolved by the combined action of ultrasonic cavitation effect and mechanical stirring. After 20 minutes, they are added to the third filter for filtration at 45°C, and the filtration accuracy is less than 7μm. After that, they are added to the first static mixer and mixed with the cotton glue solution filtered in step S2, and then added to the intermediate storage to obtain the first dispersion.

[0185] S4: adding a matting agent and a UV absorber into the first dispersion to prepare a semi-finished product;

[0186] First, the matting agent is mixed in a matting agent mixing kettle according to weight parts, filtered through a fifth filter and set aside, then the ultraviolet absorber is added to the ultraviolet absorber mixing kettle, stirred for 20 minutes, the obtained dispersion is added to the fifth filter and filtered, and then mixed with the matting agent to obtain an ultraviolet absorber-matting agent mixed liquid, and then the mixed liquid is mixed with the first dispersion in the intermediate storage in a third static mixer to obtain a semi-finished product.

[0187] S5: The semi-finished product is cast and stretched by a casting machine, and then pre-dried, peeled, dried again, and rolled up in a drying oven to obtain a cellulose triacetate film.

[0188] The mass ratio of dichloromethane to methanol in step S1 is 90:10.

[0189] The thickness of the cellulose triacetate film is 40 μm.

[0190] Comparative Example 3

[0191] A cellulose triacetate film, characterized in that, by weight, its raw materials include: 100 parts of cellulose acylate, 10 parts of plasticizer, 177 parts of solvent, 23 parts of alcohol with 1-4 carbon atoms, 1.2 parts of ultraviolet absorber, and 0.2 parts of matting agent.

[0192] The cellulose acylate is cellulose triacetate, with an acetyl substitution degree of 60.7 and a polymerization degree of 290. It was purchased from Sichuan Pushi, model number H11954.

[0193] The plasticizers are 4-biphenyloxy diphenyl phosphate and triphenyl phosphate, and the weight ratio of the two is 3:7.

[0194] The mass ratio of the cellulose acylate to the plasticizer is 100:10.

[0195] The 4-biphenyloxy diphenyl phosphate was purchased from Hubei Xinkang Pharmaceutical Chemical Co., Ltd. with a CAS number of 17269-99-7.

[0196] The triphenyl phosphate was purchased from LANXESS, Germany, with the model number being UN3077.

[0197] The ultraviolet absorber is 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl), purchased from Tianjin Lianlong, model number UV928.

[0198] The mass ratio of the plasticizer to the ultraviolet absorber is 10:1.2.

[0199] The matting agent is silicon dioxide with a particle size of 0.06 μm, purchased from Evonik of Germany, model number R972.

[0200] The solvent is dichloromethane, and the alcohol having 1 to 4 carbon atoms is methanol.

[0201] The second aspect of this embodiment provides a method for preparing a cellulose triacetate film, and the specific steps are as follows:

[0202] S1: Add alcohol with 1-4 carbon atoms by weight into a cellulose ester dissolving kettle, add cellulose acylate at a stirring speed of 700 rpm / min, stir for 2 minutes, then add dichloromethane and methanol, continue stirring for 5 minutes, and then add the cotton glue solution into the feed pump.

[0203] S2: Filter the cotton glue solution;

[0204] After the cotton glue solution in the feed pump is filtered by the first filter and the second filter, it is added to the defoaming storage for storage and standby use.

[0205] S3: mixing the plasticizer with the filtered cotton glue solution to prepare a first dispersion;

[0206] 4-Biphenyloxy diphenyl phosphate and triphenyl phosphate are added to the plasticizer mixing kettle by weight, and dispersed and dissolved by the combined action of ultrasonic cavitation effect and mechanical stirring. After 20 minutes, they are added to the third filter for filtration at 45°C, and the filtration accuracy is less than 7μm. After that, they are added to the first static mixer and mixed with the cotton glue solution filtered in step S2, and then added to the intermediate storage to obtain the first dispersion.

[0207] S4: adding a matting agent and a UV absorber into the first dispersion to prepare a semi-finished product;

[0208] First, the matting agent is mixed in a matting agent mixing kettle according to weight parts, filtered through a fifth filter and set aside, then the ultraviolet absorber is added to the ultraviolet absorber mixing kettle, stirred for 20 minutes, the obtained dispersion is added to the fifth filter and filtered, and then mixed with the matting agent to obtain an ultraviolet absorber-matting agent mixed liquid, and then the mixed liquid is mixed with the first dispersion in the intermediate storage in a third static mixer to obtain a semi-finished product.

[0209] S5: The semi-finished product is cast and stretched by a casting machine, and then pre-dried, peeled, dried again, and rolled up in a drying oven to obtain a cellulose triacetate film.

[0210] Further preferably, the mass ratio between dichloromethane and methanol in step S1 is 88:12.

[0211] The thickness of the cellulose triacetate film is 60 μm.

[0212] Comparative Example 4

[0213] The mass ratio of sugar ester compound and maleic anhydride modified ethylene-vinyl acetate was changed to 8:9, the relative molecular weight of sugar ester was changed to 300, purchased from Zhejiang Hetang Technology, model TZ-2, and the rest was the same as Example 3.

[0214] Comparative Example 5

[0215] The viscosity of maleic anhydride modified ethylene-vinyl acetate was changed to 3000 mPa.s, purchased from DIC Corporation, model 6540A, and the mass ratio of triacetylcellulose ester to plasticizer was changed to 70:10. The rest was the same as in Example 3.

[0216] Comparative Example 6

[0217] The acetyl molar percentage of the toughening agent cellulose acetate-propionate was changed to 9.0%, the propionyl molar percentage was changed to 39%, the relative molecular weight was 480, purchased from Eastman, USA, model 380A, the mass ratio of the plasticizer to the ultraviolet absorber was changed to 10:2.5, and the rest was the same as Example 3.

[0218] Performance Testing

[0219] Evaluation Method

[0220] 1. Precipitation test method

[0221] Select samples of the same weight and balance them at 85℃ and 85% humidity for 24 hours, seal and age for 500 hours, and observe the precipitation of the samples. The evaluation criteria are as follows:

[0222] 5: No precipitation

[0223] 4: A mixture of trace point precipitation and oily precipitation

[0224] 3: A small amount of fluffy precipitation and mist

[0225] 2: Part of the surface turns white in the form of snowflakes

[0226] 1: Brown snowflakes appear on the entire surface

[0227] 2. Transmittance and haze test method: Shanghai Jingke WGT-S model haze meter is used to test the transmittance and haze of cellulose triacetate film.

[0228] 3. Determination method of moisture permeability

[0229] Cut the cellulose triacetate film into a disc slightly larger than the inner diameter of the permeable cup, add desiccant and assemble the permeable cup; record the mass m1 and m2 of the permeable cup before and after being placed in the constant temperature and humidity chamber for 24 hours, and calculate the water vapor transmission rate according to the following formula. The test conditions are: temperature 40℃, relative humidity 90%.

[0230]

[0231] t—test time, h;

[0232] △m—mass increment during the test time, g; (△m=m2-m1)

[0233] A—water vapor permeability area of ​​the sample, m 2 . (28.26×10-4m 2 )

[0234] 4. Test methods for mechanical properties

[0235] The cellulose triacetate film was cut into rectangular samples with a length of 180 mm and a width of 15 mm. The length direction should be consistent with the longitudinal direction of the product. The samples were balanced for 15 hours at a temperature of 25°C and a relative humidity of 45%. The mechanical properties of the samples were tested using a WDW-5 microcomputer-controlled electronic universal testing machine.

[0236] 5. The weather resistance determination method is based on GBT-25275-2010 "Test methods for optical properties and weather resistance of polarizers for liquid crystal displays (LCD)". The optical properties, 380nm ultraviolet absorption properties, surface properties, and mechanical properties of the same sample are compared before and after aging.

[0237] 6. The dimensional stability test method is based on GBT-25275-2010 "Test methods for optical properties and weather resistance of polarizers for liquid crystal displays (LCDs)", and the horizontal and vertical shrinkage rates of the same sample are compared.

[0238] The performance comparison of each embodiment and comparative example is shown in the following table:

[0239]

[0240]

Claims

1. A cellulose triacetate film, characterized in that: The raw materials include, by weight: 80-100 parts of cellulose acylate, 5-20 parts of plasticizer, 1-10 parts of toughening agent, 100-300 parts of solvent, 10-50 parts of alcohol with 1-4 carbon atoms, 0.1-3 parts of ultraviolet absorber, and 0.1-2 parts of matting agent; The solvent is at least one of dichloromethane, chloroform, acetone, butanone, ethyl acetate, methyl acetate, propyl acetate, and butyl acetate; The plasticizer is a sugar ester compound and maleic anhydride modified ethylene-vinyl acetate, and the weight ratio of the two is (2-8): (5-8); The sugar ester compound is sucrose benzoate; The maleic anhydride modified ethylene-vinyl acetate has a viscosity of 2000-2500 mPa.s; The mass ratio of the cellulose acylate to the plasticizer is 100:(7-20).

2. A cellulose triacetate film according to claim 1, characterized in that: The relative molecular weight of the sugar ester compound is 300-1500.

3. The cellulose triacetate film according to claim 1, characterized in that: The mass ratio of the plasticizer to the ultraviolet absorber is (7-20): (0.1-1.5).

4. The cellulose triacetate film according to claim 1, characterized in that: The thickness of the cellulose triacetate film is 30-70 μm.

5. A method for preparing a cellulose triacetate film according to claim 1, characterized in that: The specific steps are as follows: S1: mixing cellulose acylate, a solvent, and an alcohol having 1 to 4 carbon atoms to prepare a cotton glue solution; S2: Filter the cotton glue solution; S3: mixing the plasticizer with the filtered cotton glue solution to prepare a first dispersion; S4: mixing the toughening agent with the first dispersion to obtain a second dispersion; S5: adding a matting agent and a UV absorber into the second dispersion to prepare a semi-finished product; S6: Casting, pre-drying, peeling, re-drying and rolling up the semi-finished product to obtain a cellulose triacetate film.