A Fe-NC MFs nanozyme and its preparation method and application

By synthesizing the catalyst for ZnHMT micron template and polymer-covered template, Fe source is introduced and carbonized at high temperature, the problem of insufficient activity and stability of Fe-N-C nanoenzymes is solved, and high performance and high stability of Fe-N-C MFs are achieved. Nanozymes, suitable for enzyme catalytic and electrocatalytic applications.

CN116116444BActive Publication Date: 2024-11-19NANJING TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211140737.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-20
Publication Date
2024-11-19
Estimated Expiration
2042-09-20

AI Technical Summary

Technical Problem

The catalytic activity and stability of existing Fe-N-C nanoenzymes are insufficient, making it difficult to meet the needs of high performance and high stability, especially in enzyme catalytic and electrocatalytic applications.

Method used

By synthesizing ZnHMT micron flower templates, polymerization reactions are carried out to form a catalyst for polymer-covered templates, Fe source is introduced for coordination, carbonize at high temperature and pickling, obtain Fe-N-C MFs nanoenzymes with flower-like structures, and enhance their oxidation-like properties. Enzyme activity and stability.

Benefits of technology

The prepared Fe-N-C MFs nanoenzymes exhibit excellent oxidase-like activity and remain stable under extreme environmental conditions, significantly improving the catalytic performance and maintaining the micron flower structure of the ZnHMT template.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116116444B_ABST
    Figure CN116116444B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of Fe-N-C micron flower (Fe-N-C MFs) nanozyme and its application. The method uses zinc-hexamethylenetetramine coordination complex (ZnHMT) as a template, firstly passes Zn 2+ The nanozyme of the present invention has the properties of oxidase, high catalytic performance, good stability and wide application range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of nanozyme catalysis technology, and specifically provides a preparation method and application of a Fe-NC MFs nanozyme. Background Art

[0002] Nanozymes are a type of nanomaterials with enzymatic properties. Like natural enzymes, they can catalyze the color change reaction of enzyme substrates and have the characteristics of enzymatic reaction kinetics. They are a new type of artificial enzyme mimics. Compared with natural enzymes, nanozymes have the advantages of high activity, good stability, low cost and easy preparation. They have broad application prospects in the fields of biosensing, environmental governance, and anti-oxidation.

[0003] In order to improve the catalytic activity of nanozymes, we simulate the active sites of natural metalloenzymes. MNC compounds (M refers to transition metals) are similar to the active sites of natural metalloenzymes M-Nx and have attracted widespread attention in recent years. The typical MNC compound Fe-NC is widely used in enzyme catalysis and electrocatalysis because it is easy to prepare and has similar active sites to natural enzymes. Therefore, the development of high-performance and high-stability Fe-NC nanozymes for colorimetric detection is still the main task at present. Summary of the invention

[0004] The purpose of the present invention is to propose a preparation and application of Fe-NC MFs nanozyme in view of the above-mentioned existing problems. First, ZnHMT micro-flowers are synthesized and used as templates to form a catalyst of polymer-coated templates by polymerization reaction, and then an Fe source is introduced to coordinate with the polymer, and then the synthesized catalyst is carbonized at high temperature to obtain a Fe-NC MFs nanozyme precursor, and finally the Fe-NC MFs nanozyme is obtained by acid washing, drying and other steps. The material presents an exquisite flower-like structure and exhibits excellent oxidase-like activity and stability.

[0005] In order to solve the technical problem of the present invention, the proposed technical solution is: a method for preparing Fe-NC MFs nanozyme, comprising the following steps:

[0006] (1) adding an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of hexamethylenetetramine, then standing the solution, centrifuging it, washing it with ethanol, and finally freeze-drying it to obtain a ZnHMT microflower template; Zn 2+ The molar ratio with HMT is 2:1;

[0007] Wherein: ZnHMT micro flower template was synthesized according to the known method and some improvements were made. 2+ The molar ratio with HMT was 2:1, and freeze drying was used instead of the previous drying method.

[0008] (2) dispersing the two monomers of the Schiff base polymer and the template synthesized in step 1 into the solution, stirring for 6 to 12 hours to obtain a catalyst of the polymer-coated template, introducing an Fe source into the polymer so that Fe and the polymer are coordinated, and the coordination reaction is carried out for 6 to 12 hours. After the reaction is completed, centrifugal drying is performed to obtain a micron flower nanozyme of a ZnHMT template coated with a Fe-doped polymer;

[0009] The polymer monomers in step (2) are p-phenylenediamine and p-benzoquinone, the mass ratio of p-phenylenediamine to p-benzoquinone is 1:0.1-5, and the amount of Fe salt added is 0.01-20mM;

[0010] The Fe salt is in the form of one of ferric chloride, ferric sulfate, and ferric acetylacetonate;

[0011] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace for high-temperature carbonization. During the carbonization process, the Fe-doped polymer and the ZnHMT template will decompose, and inorganic substances will be generated, thereby obtaining a Fe-NC MFs nanozyme precursor;

[0012] The high-temperature carbonization atmosphere in step (3) is one of nitrogen and argon, the carbonization temperature is 800-1000° C., the heating rate is 2° C. / min-5° C. / min, and the carbonization time is 1-5 h;

[0013] (4) The Fe-NC MFs nanozyme precursor obtained in step (3) is acid-washed for 6 to 12 hours to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain the Fe-NC MFs nanozyme.

[0014] (5) The catalyst obtained in step (4) was added to a buffer solution containing 3,3',5,5'-tetramethylbenzidine (TMB) and reacted at room temperature for 5 minutes.

[0015] Preferably, the solution in step (2) is one of water and ethanol.

[0016] Preferably, in step (2), the mass ratio of the two monomers of the Schiff base polymer, p-phenylenediamine and p-benzoquinone, is 1:0.1-2, and the amount of Fe salt added is 0.01-15 mM.

[0017] Preferably, the pickling solution in step (4) is 0.1 to 1 mM H 2 SO 4 One of sulfuric acid solution and 0.1-5mM HCl solution, the mass volume ratio of Fe-NC MFs nanozyme precursor to acid washing solution is 0.1-1g:50-100mL, and the acid washing temperature is 80-120℃.

[0018] Preferably, the amount of Fe salt added in step (2) is 0.1 mM, and the pickling solution in step (4) is 0.1-5 M HCl solution.

[0019] Preferably, the method comprises the following steps:

[0020] (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template;

[0021] (2) 0.54 g of p-phenylenediamine, 0.54 g of p-benzoquinone, and 1 g of ZnHMT template were dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride and stirred at 75 °C for 6 h to obtain a catalyst with a polymer-coated template. 0.1 mM FeCl 3 Add it to the polymer to coordinate Fe with the polymer, and the coordination reaction is carried out for 6 hours. After the reaction is completed, centrifuge and dry at 100°C to obtain the Fe-doped polymer-coated ZnHMT template microflower nanozyme;

[0022] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace and carbonizing it at 950°C and 5°C / min for 2 h under a nitrogen atmosphere. During the carbonization process, the Fe-doped polymer and ZnHMT template will decompose and inorganic substances will be generated, thereby obtaining a Fe-NC MFs nanozyme precursor;

[0023] (4) 1 g of the Fe-NC MFs nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100° C. for 8 h to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain the Fe-NC MFs nanozyme.

[0024] In order to solve another technical problem of the present invention, a technical solution is proposed: Fe-NC MFs nanozyme prepared according to the above method.

[0025] In order to solve another technical problem of the present invention, a technical solution is proposed: application of the Fe-NC MFs nanozyme, the Fe-NC MFs nanozyme has oxidase-like properties and can be used for catalytic reactions.

[0026] Preferably, the Fe-NC MFs nanozyme has oxidase-like properties and can be applied to the detection of some biological macromolecules and thiol substances.

[0027] The beneficial effects of the present invention are:

[0028] (1) The Fe-N-CMFs nanozyme prepared by the present invention has an exquisite flower-like structure. Fe is uniformly doped into the polymer through a coordination reaction. The method is simple to synthesize and easy to implement. In addition, with the doping of the ZnHMT template, the activity of the Fe-N-CMFs nanozyme is greatly improved.

[0029] (2) The Fe-NC MFs catalyst prepared by the present invention can exhibit excellent oxidase-like activity at room temperature, and the nanozyme remains stable under extreme environmental (temperature, pH) conditions.

[0030] (3) Figure 2 The scanning electron microscope images of the four nanozymes prepared in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 show that the Fe-NC MFs synthesized in Example 1 and the NC MFs synthesized in Comparative Example 1 maintain the original micro-flower structure of the ZnHMT template, while Comparative Examples 2 and 3 synthesized without using a template present an amorphous morphology. Figure 5 It can be seen that the oxidase-like properties of Fe-N-CMFs prepared in Example 1 of the present invention are significantly better than those of several other nanozymes.

[0031] (4) As shown in Figure (1), when FeCl is added 3 When the content of FeCl is greater than 0.1 mM, there will be a peak in the XRD spectrum, which belongs to the aggregation peak of Fe, indicating that the Fe element is not evenly dispersed in the polymer and is in a monodisperse state. Therefore, 0.1 mM FeCl 3 is the optimal amount. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 XRD patterns of Fe-NC MFs nanozymes prepared in Examples 1-6.

[0033] Figure 2 Scanning electron micrographs of the four nanozymes prepared in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3: (a) Fe-NC MFs; (b) NC MFS; (c) Fe-NC; (d) NC.

[0034] Figure 3 Transmission electron microscopy image of the Fe-NC MFs nanozyme prepared in Example 1.

[0035] Figure 4 Full XPS spectrum of the Fe-NC MFs nanozyme prepared in Example 1.

[0036] Figure 5Oxidase-like activity diagram of four nanozymes prepared in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3.

[0037] Figure 6 Catalytic activity diagram of Fe-NC MFs nanozyme prepared in Example 1 at different pH values.

[0038] Figure 7 Catalytic activity diagram of Fe-NC MFs nanozyme prepared in Example 1 at different temperatures.

[0039] Figure 8 Catalytic activity diagram of Fe-NC MFs nanozyme prepared in Example 1 at different catalyst concentrations.

[0040] Fig. 9 Stability diagram of the Fe-NC MFs nanozyme prepared in Example 1 after continuous storage in a pH 3.0 buffer solution for one week.

[0041] Fig.10 Stability diagram of the Fe-NC MFs nanozyme prepared in Example 1 stored at room temperature for three months. DETAILED DESCRIPTION

[0042] Example 1 Synthesis of Fe-NC MFs Nanozyme

[0043] (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template;

[0044] (2) 0.54 g of p-phenylenediamine, 0.54 g of p-benzoquinone, and 1 g of ZnHMT template were dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride and stirred at 75 °C for 6 h to obtain a catalyst with a polymer-coated template. 0.1 mM FeCl 3 Add it to the polymer to coordinate Fe with the polymer, and the coordination reaction is carried out for 6 hours. After the reaction is completed, centrifuge and dry at 100°C to obtain the Fe-doped polymer-coated ZnHMT template microflower nanozyme;

[0045] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace and carbonizing it at 950°C and 5°C / min for 2 h under a nitrogen atmosphere. During the carbonization process, the Fe-doped polymer and ZnHMT template will decompose and inorganic substances will be generated, thereby obtaining a Fe-NC MFs nanozyme precursor;

[0046] (4) 1 g of the Fe-NC MFs nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100° C. for 8 h to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain the Fe-NC MFs nanozyme.

[0047] Example 2 Synthesis of Fe-NC MFs Nanozyme

[0048] (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template;

[0049] (2) 0.54 g of p-phenylenediamine, 0.54 g of p-benzoquinone, and 1 g of ZnHMT template were dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride and stirred at 75 °C for 6 h to obtain a catalyst with a polymer-coated template. 1 mM FeCl 3 Add it to the polymer to coordinate Fe with the polymer, and the coordination reaction is carried out for 6 hours. After the reaction is completed, centrifuge and dry at 100°C to obtain the Fe-doped polymer-coated ZnHMT template microflower nanozyme;

[0050] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace and carbonizing it at 950°C and 5°C / min for 2 h under a nitrogen atmosphere. During the carbonization process, the Fe-doped polymer and ZnHMT template will decompose and inorganic substances will be generated, thereby obtaining a Fe-NC MFs nanozyme precursor;

[0051] (4) 1 g of the Fe-NC MFs nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100° C. for 8 h to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain the Fe-NC MFs nanozyme.

[0052] Example 3 Synthesis of Fe-NC MFs Nanozyme

[0053] (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template;

[0054] (2) 0.54 g of p-phenylenediamine, 0.54 g of p-benzoquinone, and 1 g of ZnHMT template were dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride and stirred at 75 °C for 6 h to obtain a catalyst coated with a polymer template. 3 mM FeCl 3Add it to the polymer to coordinate Fe with the polymer, and the coordination reaction is carried out for 6 hours. After the reaction is completed, centrifuge and dry at 100°C to obtain the Fe-doped polymer-coated ZnHMT template microflower nanozyme;

[0055] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace and carbonizing it at 950°C and 5°C / min for 2 h under a nitrogen atmosphere. During the carbonization process, the Fe-doped polymer and ZnHMT template will decompose and inorganic substances will be generated, thereby obtaining a Fe-NC MFs nanozyme precursor;

[0056] (4) 1 g of the Fe-NC MFs nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100° C. for 8 h to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain the Fe-NC MFs nanozyme.

[0057] Example 4 Synthesis of Fe-N-CMFs Nanozyme

[0058] (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template;

[0059] (2) 0.54 g of p-phenylenediamine, 0.54 g of p-benzoquinone, and 1 g of ZnHMT template were dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride and stirred at 75 °C for 6 h to obtain a catalyst with a polymer-coated template. 5 mM FeCl 3 Add it to the polymer to coordinate Fe with the polymer, and the coordination reaction is carried out for 6 hours. After the reaction is completed, centrifuge and dry at 100°C to obtain the Fe-doped polymer-coated ZnHMT template microflower nanozyme;

[0060] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace and carbonizing it at 950°C and 5°C / min for 2 h under a nitrogen atmosphere. During the carbonization process, the Fe-doped polymer and ZnHMT template will decompose and inorganic substances will be generated, thereby obtaining a Fe-NC MFs nanozyme precursor;

[0061] (4) 1 g of the Fe-NC MFs nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100° C. for 8 h to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain the Fe-NC MFs nanozyme.

[0062] Example 5 Synthesis of Fe-NC MFs Nanozyme

[0063] (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template;

[0064] (2) 0.54 g of p-phenylenediamine, 0.54 g of p-benzoquinone, and 1 g of ZnHMT template were dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride and stirred at 75 °C for 6 h to obtain a catalyst with a polymer-coated template. 7 mM FeCl 3 Add it to the polymer to coordinate Fe with the polymer, and the coordination reaction is carried out for 6 hours. After the reaction is completed, centrifuge and dry at 100°C to obtain the Fe-doped polymer-coated ZnHMT template microflower nanozyme;

[0065] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace and carbonizing it at 950°C and 5°C / min for 2 h under a nitrogen atmosphere. During the carbonization process, the Fe-doped polymer and ZnHMT template will decompose and inorganic substances will be generated, thereby obtaining a Fe-NC MFs nanozyme precursor;

[0066] (4) 1 g of the Fe-NC MFs nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100° C. for 8 h to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain the Fe-NC MFs nanozyme.

[0067] Example 6 Synthesis of Fe-NC MFs Nanozyme

[0068] (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template;

[0069] (2) 0.54 g of p-phenylenediamine, 0.54 g of p-benzoquinone, and 1 g of ZnHMT template were dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride and stirred at 75 °C for 6 h to obtain a catalyst coated with a polymer template. 10 mM FeCl 3 Add it to the polymer to coordinate Fe with the polymer, and the coordination reaction is carried out for 6 hours. After the reaction is completed, centrifuge and dry at 100°C to obtain the Fe-doped polymer-coated ZnHMT template microflower nanozyme;

[0070] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace and carbonizing it at 950°C and 5°C / min for 2 h under a nitrogen atmosphere. During the carbonization process, the Fe-doped polymer and ZnHMT template will decompose and inorganic substances will be generated, thereby obtaining a Fe-NC MFs nanozyme precursor;

[0071] (4) 1 g of the Fe-NC MFs nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100° C. for 8 h to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain the Fe-NC MFs nanozyme.

[0072] As shown in Figure (1), when FeCl is added 3 When the content of FeCl is greater than 0.1 mM, there will be a peak in the XRD spectrum, which belongs to the aggregation peak of Fe, indicating that the Fe element is not evenly dispersed in the polymer and is in a monodisperse state. Therefore, 0.1 mM FeCl 3 is the optimal amount.

[0073] Example 7 Synthesis of Fe-NC MFs Nanozyme

[0074] (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template;

[0075] (2) 0.54 g of p-phenylenediamine, 1.08 g of p-benzoquinone, and 1 g of ZnHMT template were dispersed in an aqueous solution containing 0.075 g of zinc chloride and stirred at 75 °C for 12 h to obtain a catalyst with a polymer-coated template. 0.1 mM FeCl 3 Add it to the polymer to coordinate Fe with the polymer, and the coordination reaction lasts for 12 hours. After the reaction is completed, centrifuge and dry at 100°C to obtain the Fe-doped polymer-coated ZnHMT template microflower nanozyme;

[0076] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace and carbonizing it at 800°C and 2.5°C / min for 4 h under nitrogen atmosphere. During the carbonization process, the Fe-doped polymer and ZnHMT template will decompose and inorganic substances will be generated to obtain Fe-NC MFs nanozyme precursor;

[0077] (4) 1 g of Fe-NC MFs nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100 °C for 4 h to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain Fe-N-CMFs nanozyme.

[0078] Example 8 Synthesis of Fe-NC MFs Nanozyme

[0079] (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template;

[0080] (2) 1.08 g of p-phenylenediamine, 0.54 g of p-benzoquinone and 1 g of ZnHMT template were dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride, and stirred at 75° C. for 8 h to obtain a catalyst of a polymer-coated template. 0.1 mM of ferric sulfate was added to the polymer to coordinate Fe with the polymer. The coordination reaction lasted for 8 h. After the reaction was completed, the reaction was centrifuged and dried at 100° C. to obtain a Fe-doped polymer-coated ZnHMT template microflower nanozyme.

[0081] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace and carbonizing it at 1000°C and 3°C / min for 5 h under a nitrogen atmosphere. During the carbonization process, the Fe-doped polymer and ZnHMT template will decompose and inorganic substances will be generated, thereby obtaining a Fe-NC MFs nanozyme precursor;

[0082] (4) The 0.5 g Fe-NC MFs nanozyme precursor obtained in step (3) was acid-washed in 80 mL 1 M hydrochloric acid solution at 100 ° C for 8 h to remove the metal Fe oxide, and then centrifuged, washed, and dried to obtain Fe-N-CMFs nanozyme.

[0083] Example 9 Synthesis of Fe-NC MFs Nanozyme

[0084] (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template;

[0085] (2) 0.54 g of p-phenylenediamine, 0.54 g of p-benzoquinone and 1 g of ZnHMT template were dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride, and stirred at 75° C. for 6 h to obtain a catalyst of a polymer-coated template. 0.1 mM of ferric acetylacetonate was added to the polymer to coordinate Fe with the polymer. The coordination reaction lasted for 6 h. After the reaction was completed, the reaction was centrifuged and dried at 100° C. to obtain a Fe-doped polymer-coated ZnHMT template microflower nanozyme.

[0086] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace and carbonizing it at 900°C and 4°C / min for 3 h under nitrogen atmosphere. During the carbonization process, the Fe-doped polymer and ZnHMT template will decompose and inorganic substances will be generated to obtain Fe-NC MFs nanozyme precursor;

[0087] (4) 1 g of Fe-NC MFs nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 0.5 M sulfuric acid solution at 100 ° C for 8 h to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain Fe-N-CMFs nanozyme. The sulfuric acid solution used as the acid washing solution cannot remove Fe impurities, so the most preferred acid washing solution is hydrochloric acid solution as the acid washing solution.

[0088] Example 10 Fe-NC MFs nanozyme oxidase activity, catalytic conditions and stability test

[0089] (1) Example (1) The synthesized Fe-NC MFs-type oxidase catalytic reaction system comprises 5 μg / mL Fe-NC, HAc-NaAc buffer solution of pH 3.0, and 0.4 mM TMB. After reacting at room temperature for 5 min, the absorbance value of the system within 500-800 nm is tested by UV-visible spectrophotometer;

[0090] (2) Based on experiment (1), we screened the catalytic conditions of Fe-NC MFs nanozymes and obtained the optimal catalytic conditions by testing the enzyme activity under the conditions of pH 2.0-10.0, temperature 0-100°C, and catalyst concentration 0-20 μg / mL. Figure 6 , 7 The catalyst shown has the highest activity at pH 3.0 and temperature 45°C, and we can find that the catalytic activity of the catalyst can reach more than 95% at room temperature, so we choose to carry out subsequent experiments at room temperature;

[0091] (3) The Fe-NC MFs nanozyme was stored in a buffer solution of pH 3.0, and based on experiment (1), the enzyme activity change of the catalyst was tested by UV-visible spectrophotometer for one week; as an exception, the solid catalyst was stored at room temperature for three months, and based on experiment (1), the enzyme activity change was tested by UV-visible spectrophotometer to further confirm the stability of the catalyst.

[0092] Comparative Example 1

[0093] Comparative Example 1 provides a method for preparing NC MFs nanozymes, and the specific steps are as follows:

[0094] (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template;

[0095] (2) Dispersing 0.54 g of p-phenylenediamine, 0.54 g of p-benzoquinone and 1 g of ZnHMT template into an anhydrous ethanol solution containing 0.075 g of zinc chloride, stirring at 75° C. for 12 h, obtaining a catalyst coated with a polymer template, centrifuging after the reaction, and drying at 100° C. to obtain a polymer-coated ZnHMT template microflower nanozyme;

[0096] (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace, and performing high temperature carbonization at 950° C. and 5° C. / min for 2 h under nitrogen atmosphere to obtain a NC micron flower nanozyme precursor;

[0097] (4) 1 g of NC microflower nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100° C. for 8 h, and then centrifuged, washed, and dried to obtain NC MFs nanozyme.

[0098] Comparative Example 2

[0099] Comparative Example 2 provides a method for preparing Fe-NC nanozyme, and the specific steps are as follows:

[0100] (1) 0.54 g of p-phenylenediamine and 0.54 g of p-benzoquinone were dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride. The two monomers were polymerized and stirred at 75 °C for 6 h. 0.1 mM FeCl 3 Add it to the polymer to coordinate Fe with the polymer, and the coordination reaction is carried out for 6 hours. After the reaction is completed, centrifuge and dry at 100°C to obtain the Fe-doped polymer nanozyme;

[0101] (2) placing the nanozyme precursor obtained in step 1 in a tubular furnace and carbonizing it at 950° C. and 5° C. / min for 2 h under a nitrogen atmosphere. During the carbonization process, the Fe-doped polymer will decompose and inorganic substances will be generated, thereby obtaining a Fe-NC nanozyme precursor;

[0102] (4) 1 g of the Fe-NC nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100° C. for 8 h to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain the Fe-NC nanozyme.

[0103] Comparative Example 3

[0104] Comparative Example 3 provides a method for preparing NC nanozyme, and the specific steps are as follows:

[0105] (1) 0.54 g of p-phenylenediamine and 0.54 g of p-benzoquinone are dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride, and the two monomers are polymerized. The mixture is stirred at 75° C. for 12 h. After the reaction is completed, the mixture is centrifuged and dried at 100° C. to obtain a polymer nanozyme.

[0106] (2) placing the nanozyme precursor obtained in step 1 in a tubular furnace and carbonizing it at 950° C. and 5° C. / min for 2 h under a nitrogen atmosphere. During the carbonization process, the polymer will decompose and inorganic substances will be generated to obtain a NC nanozyme precursor;

[0107] (4) 1 g of NC nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100° C. for 8 h, and then centrifuged, washed, and dried to obtain NC nanozyme.

Claims

1. A method for preparing Fe-NC MFs nanozyme, Features: The following steps are involved: (1) adding an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of hexamethylenetetramine, then standing the solution, centrifuging it, washing it with ethanol, and finally freeze-drying it to obtain a ZnHMT microflower template; Zn 2+ The molar ratio with HMT is 2:1; (2) dispersing the two monomers of the Schiff base polymer and the template synthesized in step 1 into the solution, stirring for 6 to 12 hours to obtain a catalyst of the polymer-coated template, introducing Fe salt into the polymer to coordinate Fe with the polymer, and the coordination reaction lasts for 6 to 12 hours. After the reaction is completed, centrifugal drying is performed to obtain a micron flower nanozyme of ZnHMT template coated with Fe doped polymer; The polymer monomers in step (2) are p-phenylenediamine and p-benzoquinone, the mass ratio of p-phenylenediamine to p-benzoquinone is 1:0.1-5, and the amount of Fe salt added is 0.01-20mM; The Fe salt is in the form of one of ferric chloride, ferric sulfate, and ferric acetylacetonate; (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace for high-temperature carbonization. During the carbonization process, the Fe-doped polymer and the ZnHMT template will decompose, and inorganic substances will be generated, thereby obtaining a Fe-NC MFs nanozyme precursor; The high-temperature carbonization atmosphere in step (3) is one of nitrogen and argon, the carbonization temperature is 800-1000° C., the heating rate is 2° C. / min-5° C. / min, and the carbonization time is 1-5 h; (4) The Fe-NC MFs nanozyme precursor obtained in step (3) is acid-washed for 6 to 12 hours to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain the Fe-NC MFs nanozyme.

2. The method for preparing Fe-NC MFs nanozyme according to claim 1, Features: The solution in step (2) is one of water and ethanol.

3. The method for preparing Fe-NC MFs nanozyme according to claim 1, Features: In step (2), the mass ratio of the two monomers of the Schiff base polymer, p-phenylenediamine and p-benzoquinone, is 1:0.1-2, and the amount of Fe salt added is 0.01-15mM.

4. The method for preparing Fe-NC MFs nanozyme according to claim 1, Features: Step (4) The pickling solution is 0.1-1 mM H 2 SO 4 One of sulfuric acid solution or 0.1-5mM HCl solution, the mass volume ratio of Fe-NC MFs nanozyme precursor to acid washing solution is 0.1-1g:50-100mL, and the acid washing temperature is 80-120℃.

5. The method for preparing Fe-NC MFs nanozyme according to claim 1, Features: The amount of Fe salt added in step (2) is 0.1 mM, and the pickling solution in step (4) is 0.1-5 M HCl solution.

6. The method for preparing Fe-NC MFs nanozyme according to claim 1, Features: The following steps are involved: (1) adding 1.06 g of an ethanol solution of zinc nitrate hexahydrate to an ethanol solution of 0.25 g of hexamethylenetetramine, and then standing for 1 hour, centrifuging, washing with ethanol, and finally freeze-drying to obtain a ZnHMT microflower template; (2) 0.54 g of p-phenylenediamine, 0.54 g of p-benzoquinone, and 1 g of ZnHMT template were dispersed in an anhydrous ethanol solution containing 0.075 g of zinc chloride and stirred at 75 °C for 6 h to obtain a catalyst with a polymer-coated template. 0.1 mM FeCl 3 Add it to the polymer to coordinate Fe with the polymer, and the coordination reaction is carried out for 6 hours. After the reaction is completed, centrifuge and dry at 100°C to obtain the Fe-doped polymer-coated ZnHMT template microflower nanozyme; (3) placing the micron flower nanozyme precursor obtained in step 2 in a tubular furnace and carbonizing it at 950°C and 5°C / min for 2 h under a nitrogen atmosphere. During the carbonization process, the Fe-doped polymer and ZnHMT template will decompose and inorganic substances will be generated, thereby obtaining a Fe-NC MFs nanozyme precursor; (4) 1 g of the Fe-NC MFs nanozyme precursor obtained in step (3) was acid-washed in 80 mL of 1 M hydrochloric acid solution at 100° C. for 8 h to remove metal Fe oxides, and then centrifuged, washed, and dried to obtain the Fe-NC MFs nanozyme.

7. The Fe-NC MFs nanozyme prepared according to any one of claims 1-6.

8. The use of the Fe-NC MFs nanozyme according to claim 7, Features: Fe-N-CMFs nanozymes have oxidase-like properties and are used to catalyze reactions.

9. The use of the Fe-NC MFs nanozyme according to claim 7, Features: Fe-N-CMFs nanozymes have oxidase-like properties and are used in the detection of some biological macromolecules and thiol substances.