Zinc alloy welding sheet for copper-clad aluminum butt welding, preparation method, and welding method
Preparation through arc melting, quench-swinging belt and laser remelting methods of zinc alloy welding sheets, the problems of low joint strength and defects in copper-clad aluminum welding are solved, and high-quality copper-clad aluminum welding is achieved to meet the application needs of the power industry. .
Patent Information
- Application Number
- CN202310167489.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-02-27
AI Technical Summary
During the copper-clad aluminum welding process, due to the difference in melting points between copper and aluminum, the outer copper layer is not welded when the welding temperature is higher than the aluminum melting point, and the inner aluminum layer melts prematurely when it is lower than the copper melting point, resulting in low joint strength and easy heat occurrence Cracked and inclusion defects, the strength of existing tin soldering materials is not sufficient to meet the application needs of the power industry.
The zinc alloy welding sheet is used, which consists of zinc, aluminum, copper, magnesium, gadolinium and other elements. The zinc alloy welding sheet with a micron-level rough surface is prepared by arc melting, quenching belt and laser remelting method, and the lower melting point of zinc is used. Welding is carried out below the melting point of aluminum to increase the affinity of zinc alloy with copper and aluminum, and purify grain boundaries by magnesium and gadolinium to improve welding uniformity and wetting.
Copper-clad aluminum welding is achieved below the aluminum melting point, avoiding thermal cracks and inclusion defects, improving the strength and consistency of the joints, and meeting the power industry's demand for high-quality welding.
Smart Images

Figure CN116117380B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a zinc alloy welding piece for copper-clad aluminum butt welding and a preparation method and a welding method of the aluminum alloy welding piece, belonging to the technical field of solder. Background Art
[0002] Copper clad aluminum is a material that is coated with copper on the outer surface of aluminum. The metallurgical bonding at the interface between copper and aluminum is used to form a solid and reliable integral material with two different metal materials, such as copper clad aluminum wire, copper clad aluminum busbar, and copper clad aluminum rod. Copper clad aluminum has both the high conductivity of copper and the low density of aluminum. It can not only ensure electrical performance but also save material costs. It has broad application prospects in signal transmission and power transmission. In actual industrial applications, copper clad aluminum welding is often required to facilitate the normal operation of the entire equipment. When copper clad aluminum welding is performed, the outer layer of copper and copper, and the inner layer of aluminum and aluminum need to be welded before the entire copper clad aluminum can be welded. The melting point of copper is 1083℃, and the melting point of aluminum is 660℃. The melting points of the two metal materials are very different. When the welding temperature is higher than the melting point of aluminum and lower than the melting point of copper, the inner layer of aluminum will be welded on the copper clad aluminum welding surface, but the outer layer of copper will not be welded, and the overall strength of the copper clad aluminum joint is low. When the welding temperature is higher than the melting point of copper, the premature melting of the inner aluminum will corrode the outer copper, which will not only reduce the welding of the outer copper, but also cause corrosion problems in the inner aluminum. More importantly, the melting of aluminum in copper-clad aluminum welding will cause defects such as thermal cracks and inclusions, reducing the strength of the joint. Therefore, using a welding temperature below the melting point of aluminum is an important condition that needs to be considered in copper-clad aluminum welding.
[0003] Chinese patents CN103056250A and CN112589223A disclose methods for welding copper-clad aluminum wires. Both welding methods use tin as the welding material. The melting point of tin is 231.9°C, which is much lower than the melting points of copper and aluminum. Copper and aluminum remain in a solid state during the soldering process. After the tin melts, it wets the surface of the copper-clad aluminum wire and then cools to achieve the welding of the copper-clad aluminum wire. Although tin can complete the welding of the outer copper layer of the copper-clad aluminum wire and the inner aluminum layer of the copper-clad aluminum wire, the strength of tin is low, and the strength of the copper-clad aluminum joint welded by it is also low, which does not meet the application requirements of the power industry for current transmission. Summary of the invention
[0004] In order to better achieve the welding of copper-clad aluminum materials, the present invention provides a zinc alloy welding sheet for copper-clad aluminum butt welding. The zinc alloy welding sheet has a thickness of 30μm-50μm and is composed of the following elements in parts by weight: 80-92 parts of zinc, 2-8 parts of aluminum, 2-8 parts of copper, 2-3 parts of magnesium, 0.5-1.5 parts of niobium, and 0.5-1.5 parts of gadolinium.
[0005] Wherein, aluminum and niobium are added in the form of aluminum-niobium alloy, and aluminum and gadolinium are added in the form of aluminum-gadolinium alloy.
[0006] The preparation method of the zinc alloy welding sheet for copper-clad aluminum butt welding of the present invention is as follows: 1) corresponding metal particles or alloy particles are weighed according to the element ratio, mixed evenly and then melted by electric arc to obtain a block mother alloy; 2) the block mother alloy obtained in step 1) is heated to 380-450° C. to melt, and the mother alloy is made into a zinc alloy foil strip by a rapid cooling strip spinning method; 3) the zinc alloy foil strip obtained in step 2) is treated by a laser remelting method to obtain a micron-level rough surface, thereby obtaining the zinc alloy welding sheet.
[0007] The arc melting method, rapid cooling strip throwing method and laser remelting method used in the above method can all be carried out using existing processes, and the specific parameters are controlled as follows:
[0008] Arc process parameters: vacuum degree 0.01~0.05Pa, arc voltage 20~30V, arc current 20~30A.
[0009] Rapid cooling and strip spinning process parameters: rapid cooling and strip spinning speed is 1200-1600rpm, and blowing argon pressure is 0.3-0.6MPa.
[0010] Laser remelting process parameters: laser power 50-100W, scanning speed 500-600mm / s, scanning spacing 50-60μm.
[0011] The zinc alloy welding sheet of the present invention is specially used for welding copper-clad aluminum weldments. The specific steps are: placing the zinc alloy welding sheet between the welding surfaces of the copper-clad aluminum weldments, pressurizing by 3-5 MPa, induction heating until the zinc alloy welding sheet melts, and short-term heat preservation for 1-4 seconds to complete welding.
[0012] The copper-clad aluminum weldments referred to in the present invention specifically include copper-clad aluminum wires, copper-clad aluminum bars, copper-clad aluminum rods, copper-clad aluminum plates, copper-clad aluminum strips, and the like, which have welds that can accommodate the zinc alloy welding pieces of the present invention.
[0013] The zinc alloy welding sheet of the present invention has the following advantages: zinc with a melting point of 419° C. is used as a matrix element, and copper-clad aluminum welding is performed at a welding temperature lower than the melting point of aluminum, thereby avoiding defects such as thermal cracks, pores and inclusions caused by high welding temperatures; the added aluminum and copper elements can increase the affinity of the zinc alloy with the outer copper layer and the inner aluminum layer, and improve the wettability of the zinc alloy with the outer copper layer and the inner aluminum layer; the magnesium element in the zinc alloy can remove the oxide scale on the surface of the outer copper layer and the inner aluminum layer, and solve the problem that the oxide scale weakens the wettability of the zinc alloy; niobium and gadolinium elements have the functions of purifying grain boundaries and refining grains, and can promote the uniformity of the zinc alloy phase structure, which is beneficial to welding uniformity; the rough micron-level organizational structure on the surface of the zinc alloy can improve the diffusion driving force of the alloy elements and increase the wettability of the zinc alloy.
[0014] Compared with the prior art, the zinc alloy welding sheet of the present invention has excellent wettability, can simultaneously realize the welding of the outer copper layer and the inner aluminum layer, ensure the welding consistency of the copper-clad aluminum joint, obtain a high-strength copper-clad aluminum joint, and can be widely used in the high-quality welding of copper-clad aluminum buses or copper-clad aluminum rods in the power industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 The microstructure of the surface of the zinc alloy welding piece in Example 1;
[0016] Figure 2 This is a microscopic photograph of the weld of a copper-clad aluminum bar welded with the zinc alloy welding sheet of Example 1, wherein the numbers are: 1, aluminum layer, 2, welding layer, 3, copper layer. DETAILED DESCRIPTION
[0017] The following embodiments, in conjunction with the accompanying drawings, are only intended to illustrate the technical solutions described in the claims and are not intended to limit the protection scope of the claims.
[0018] Example 1
[0019] A zinc alloy welding sheet for copper-clad aluminum butt welding has a thickness of 30 μm and comprises the following elements in parts by weight: 85 parts of zinc, 5 parts of aluminum, 5 parts of copper, 2.5 parts of magnesium, 1 part of niobium, and 1 part of gadolinium, wherein aluminum and niobium are added in the form of aluminum-niobium alloy, and aluminum and gadolinium are added in the form of aluminum-gadolinium alloy.
[0020] The preparation method of the zinc alloy welding sheet for copper-clad aluminum butt welding in this embodiment is as follows:
[0021] 1) According to the element ratio, corresponding metal particles or alloy particles are weighed, mixed evenly, and then arc-melted to obtain a block master alloy. The arc process parameters are: vacuum degree 0.03Pa, arc voltage 25V, arc current 25A;
[0022] 2) heating the master alloy block obtained in step 1) to 420° C. to melt, and using a quenching strip spinning method to make the master alloy into a zinc alloy foil strip, wherein the quenching strip spinning speed is 1400 rpm and the blowing argon pressure is 0.5 MPa;
[0023] 3) The zinc alloy foil strip obtained in step 2) is processed by laser remelting to obtain a micrometer-level rough surface, that is, the zinc alloy welding sheet is obtained; the process control of the laser remelting method is: laser power 75W, scanning speed 550mm / s, scanning spacing 55μm.
[0024] Example 2
[0025] A zinc alloy welding sheet for copper-clad aluminum butt welding has a thickness of 50 μm and comprises the following elements in parts by weight: 80 parts of zinc, 8 parts of aluminum, 8 parts of copper, 2 parts of magnesium, 0.5 parts of niobium, and 1.5 parts of gadolinium, wherein aluminum and niobium are added in the form of aluminum-niobium alloy, and aluminum and gadolinium are added in the form of aluminum-gadolinium alloy.
[0026] The preparation method of the zinc alloy welding sheet for copper-clad aluminum butt welding in this embodiment is as follows:
[0027] 1) According to the element ratio, the corresponding metal particles or alloy particles are weighed, mixed evenly, and then arc-melted to obtain a block master alloy. The arc process parameters are: vacuum degree 0.05Pa, arc voltage 30V, arc current 20A;
[0028] 2) heating the master alloy block obtained in step 1) to 450° C. to melt, and using a quenching strip spinning method to make the master alloy into a zinc alloy foil strip, wherein the quenching strip spinning speed is 1600 rpm and the blowing argon pressure is 0.6 MPa;
[0029] 3) The zinc alloy foil strip obtained in step 2) is processed by laser remelting to obtain a micron-level rough surface, that is, the zinc alloy welding sheet is obtained; the process control of the laser remelting method is: laser power 100W, scanning speed 600mm / s, scanning spacing 50μm.
[0030] Example 3
[0031] A zinc alloy welding sheet for copper-clad aluminum butt welding has a thickness of 40 μm and comprises the following elements in parts by weight: 92 parts of zinc, 2 parts of aluminum, 2 parts of copper, 3 parts of magnesium, 1.5 parts of niobium, and 0.5 parts of gadolinium, wherein aluminum and niobium are added in the form of aluminum-niobium alloy, and aluminum and gadolinium are added in the form of aluminum-gadolinium alloy.
[0032] The preparation method of the zinc alloy welding sheet for copper-clad aluminum butt welding in this embodiment is as follows:
[0033] 1) According to the element ratio, the corresponding metal particles or alloy particles are weighed, mixed evenly, and then arc-melted to obtain a block master alloy. The arc process parameters are: vacuum degree 0.01Pa, arc voltage 20V, arc current 30A;
[0034] 2) heating the master alloy block obtained in step 1) to 380° C. to melt, and using a quenching strip spinning method to make the master alloy into a zinc alloy foil strip, wherein the quenching strip spinning speed is 1200 rpm and the blowing argon pressure is 0.3 MPa;
[0035] 3) The zinc alloy foil strip obtained in step 2) is processed by laser remelting to obtain a micron-level rough surface, that is, the zinc alloy welding sheet is obtained; the process control of the laser remelting method is: laser power 50W, scanning speed 500mm / s, scanning spacing 60μm.
[0036] Example 4
[0037] A zinc alloy welding sheet for copper-clad aluminum butt welding has a thickness of 45 μm and is composed of the following elements in parts by weight: 90 parts of zinc, 3 parts of aluminum, 5 parts of copper, 3 parts of magnesium, 1 part of niobium, and 1.5 parts of gadolinium, wherein aluminum and niobium are added in the form of aluminum-niobium alloy, and aluminum and gadolinium are added in the form of aluminum-gadolinium alloy.
[0038] The preparation method of the zinc alloy welding sheet for copper-clad aluminum butt welding in this embodiment is as follows:
[0039] 1) According to the element ratio, the corresponding metal particles or alloy particles are weighed, mixed evenly, and then arc-melted to obtain a block master alloy. The arc process parameters are: vacuum degree 0.03Pa, arc voltage 30V, arc current 22A;
[0040] 2) heating the master alloy block obtained in step 1) to 400° C. to melt, and using a quenching strip spinning method to make the master alloy into a zinc alloy foil strip, wherein the quenching strip spinning speed is 1500 rpm and the blowing argon pressure is 0.5 MPa;
[0041] 3) The zinc alloy foil strip obtained in step 2) is processed by laser remelting to obtain a micrometer-level rough surface, that is, the zinc alloy welding sheet is obtained; the process control of the laser remelting method is: laser power 80W, scanning speed 600mm / s, scanning spacing 55μm.
[0042] Figure 1 This is the microstructure of the surface of the zinc alloy welding piece obtained in Example 1. It can be seen that the surface of the welding piece obtained in Example 1 is evenly distributed with grooves, forming a scaly surface microstructure. During induction heating, the raised scale points can melt quickly, and the grooves can also guide the gas out, thereby forming a dense weld with the weldment.
[0043] Figure 2 The weld microscopic photo of the copper-clad aluminum bar welded by the zinc alloy welding piece in Example 1 is as follows: the zinc alloy welding piece is placed between the welding surfaces of the copper-clad aluminum bar welded piece, pressurized to 5MPa, induction heated to 430℃ to melt the zinc alloy welding piece, and kept warm for 2s to complete the welding. It can be seen that the welding layer 2 is uniform and dense, with a thickness of about 25μm, and the welding layer is fully in contact with the aluminum layer 1 and the copper layer 3. The welding layer fills the micro-depressions on the surface of the aluminum layer 1 and the copper layer 3, achieving good welding of the copper-clad aluminum bar welded piece.
[0044] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a zinc alloy welding sheet for copper-clad aluminum butt welding, It is characterized in that The zinc alloy welding sheet for copper-clad aluminum butt welding is characterized in that the zinc alloy welding sheet has a thickness of 30 μm to 50 μm and comprises the following elements in parts by weight: 80 to 92 parts of zinc, 2 to 8 parts of aluminum, 2 to 8 parts of copper, 2 to 3 parts of magnesium, 0.5 to 1.5 parts of niobium, and 0.5 to 1.5 parts of gadolinium; The aluminum and niobium are added in the form of aluminum-niobium alloy; the aluminum and gadolinium are added in the form of aluminum-gadolinium alloy; The method for preparing the zinc alloy welding sheet for copper-clad aluminum butt welding comprises the following steps: 1) According to the element ratio, the corresponding metal particles or alloy particles are weighed, mixed evenly, and then arc-melted to obtain a bulk master alloy; 2) heating the master alloy block obtained in step 1) to 380-450° C. to melt the master alloy, and using a rapid cooling strip spinning method to make a zinc alloy foil strip; 3) The zinc alloy foil strip obtained in step 2) is processed by laser remelting to obtain a micron-level rough surface, thereby obtaining the zinc alloy welding sheet.
2. The method according to claim 1, It is characterized in that In step 1), arc process parameters are: vacuum degree 0.01~0.05Pa, arc voltage 20~30V, arc current 20~30A.
3. The method according to claim 1, It is characterized in that In step 2), the quenching belt rotation speed is 1200-1600 rpm, and the blowing argon pressure is 0.3-0.6 MPa.
4. The method according to claim 1, It is characterized in that In step 3), the laser remelting process is controlled as follows: laser power 50-100 W, scanning speed 500-600 mm / s, and scanning spacing 50-60 μm.
5. A method for welding a copper-clad aluminum weldment, It is characterized in that The zinc alloy welding sheet for copper-clad aluminum butt welding obtained according to any one of claims 1 to 4 is used for welding, the zinc alloy welding sheet is placed between the welding surfaces of the copper-clad aluminum weldment, pressurized to 3 to 5 MPa, induction heated until the zinc alloy welding sheet melts, and briefly kept warm for 1 to 4 seconds to complete the welding.
6. The method for welding a copper-clad aluminum weldment according to claim 5, It is characterized in that The copper-clad aluminum weldment is selected from one of a copper-clad aluminum wire, a copper-clad aluminum bar, a copper-clad aluminum rod, a copper-clad aluminum plate, and a copper-clad aluminum strip.
Citation Information
Patent Citations
Welding method of copper-clad aluminum enameled wire
CN103056250A
Copper-clad aluminum flat wire welding device
CN112589223A
Soldering lug for soft soldering and power module assembly structure
CN103769764A
Tin-based composite material preformed soldering lug for power chip packaging and preparation method of tin-based composite material preformed soldering lug
CN115008060A
Alloy composition and method for low temperature fluxless brazing
CN1615204A