A degradable packaging film and preparation method thereof
Through the combination of the two-layer structure and specific materials, the mechanical properties of the degradable packaging film are improved, the problem of insufficient mechanical properties of the existing packaging film is solved, and efficient mechanical properties and environmentally friendly degradation effects are achieved.
Patent Information
- Application Number
- CN202310114036.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-15
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-02-15
AI Technical Summary
The existing degradable packaging film has poor mechanical properties such as tensile strength, elongation of break and puncture resistance, which limits its promotion and use.
A packaging film with a double-layer structure, in which the outer layer consists of polybutylene succinate, polyethylene, sodium alginate, coconut palm fiber and nano zinc oxide, and the inner layer is composed of modified starch, chitosan, sugarcane fiber It is composed of talc powder and connected by adhesive, combined with pretreatment of coconut palm fiber and preparation method of modified starch to improve mechanical properties.
It significantly improves the tensile strength, elongation of break and puncture resistance of the packaging film, while maintaining degradability, enhancing environmentally friendly mechanical properties and degradation properties.
Smart Images

Figure BDA0004077842900000091 
Figure BDA0004077842900000101
Abstract
Description
Technical Field
[0001] The present application relates to the field of plastic film products, and in particular to a degradable packaging film and a preparation method thereof. Background Art
[0002] White pollution refers to the pollution caused to the environment by waste plastics. Waste plastics mainly include packaging bags, agricultural mulch films, disposable tableware, plastic bottles and other plastic products. These plastic products are usually made of high molecular compounds such as polystyrene, polypropylene, and polyvinyl chloride. Since these plastic products are difficult to degrade, if they are thrown away at will, they will cause pollution to the ecological environment and landscape.
[0003] In recent years, with the improvement of people's environmental awareness, the problem of white pollution has become the focus of social attention. Biodegradable materials are usually used to prepare packaging films to replace plastic products, which effectively alleviates the problem of white pollution. In the relevant technology, biodegradable products include films made of polysaccharides such as cellulose, modified starch, sodium alginate, chitosan, etc. These films are used for fruit preservation and food packaging. Recycled films can be centrally processed for degradation without pollution to the environment.
[0004] However, the mechanical properties of this type of film products, such as tensile strength, elongation at break and puncture resistance, are poor, which limits their promotion and use. Summary of the invention
[0005] In order to improve the problem of poor mechanical properties such as tensile strength, elongation at break and puncture resistance of degradable packaging films, the present application provides a degradable packaging film and a preparation method thereof.
[0006] The present application provides a degradable packaging film, which adopts the following technical solution:
[0007] A degradable packaging film, comprising an outer layer and an inner layer, wherein the outer layer comprises the following raw materials in parts by weight: 35-50 parts of polybutylene succinate, 20-30 parts of polyethylene, 15-20 parts of polyvinyl alcohol, 5-9 parts of sodium alginate, 4-8 parts of coconut palm fiber, 3-5 parts of plasticizer, and 14-18 parts of nano zinc oxide;
[0008] The inner layer comprises the following raw materials in parts by weight: 20-30 parts of modified starch, 5-15 parts of chitosan, 2-4 parts of emulsifier, 8-12 parts of sugarcane fiber, 1-3 parts of nano titanium dioxide, 3-5 parts of plasticizer, and 12-16 parts of talc; wherein the outer layer and the inner layer are connected by an adhesive.
[0009] By adopting the above technical scheme, the raw materials of the outer layer and the inner layer are both made of degradable materials, which are environmentally friendly. In addition, among the raw materials of the outer layer, polybutylene succinate has excellent mechanical properties and heat resistance, and can eventually be degraded into small molecules such as carbon dioxide, water and methane under the action of natural microorganisms. Polyethylene has good transparency, abrasion resistance and impact resistance. Polyvinyl alcohol has good transparency, high tensile strength and good thermal insulation. The mixture of polybutylene succinate, polyethylene and polyvinyl alcohol improves the mechanical properties of the packaging film such as tensile strength, elongation at break and abrasion resistance.
[0010] Sodium alginate has good biocompatibility. Sodium alginate is mixed with polyethylene and polyvinyl alcohol to increase the toughness, elongation at break and tensile strength of the packaging film. The outer surface of coconut palm fiber is rough and porous, and is arranged in a three-dimensional network pattern. It has greater elasticity and good wear resistance. Nano zinc oxide is loaded in the pore structure of coconut palm fiber, which increases the structural strength of coconut palm fiber and has good UV resistance and bactericidal properties. Sodium alginate has a certain viscosity and is coated on the outer surface of coconut palm fiber, thereby increasing the adhesion between nano zinc oxide and coconut palm fiber, and further increasing the structural strength and mechanical properties of the packaging film.
[0011] The inner layer adopts modified starch, which has good degradability. The modified starch and chitosan are mixed to prepare the film. There are a large number of active hydroxyl groups and amino groups in the chitosan molecules. They have strong chemical reaction ability and strong anion adsorption capacity. They combine with the molecules in the modified starch to form a three-dimensional network structure, which enhances the interaction between the membrane molecular chains and greatly enhances the tensile capacity of the film, so that the prepared film has good mechanical properties. Sugarcane fiber has good antibacterial and toughness. Sugarcane fiber is dispersed in the network structure formed by chitosan and modified starch, which increases the structural strength and toughness of the inner film, thereby improving the mechanical properties of the inner layer.
[0012] By setting up a double layer of outer layer and inner layer, the mechanical properties of the packaging film such as tensile strength, elongation at break and puncture resistance are increased, which not only makes the packaging film easy to degrade but also has better mechanical properties.
[0013] Preferably, the coconut palm fiber is pretreated, comprising the following steps:
[0014] (1) soaking coconut palm fiber in a NaOH solution, and then washing with deionized water to neutralize it, to obtain alkali-treated coconut palm fiber; (2) mixing the alkali-treated coconut palm fiber obtained in step (1) with epoxy resin, and then adding nano-microcrystalline cellulose and konjac gum, stirring at 60-80° C. for 1-2 hours, and freeze-drying to obtain pretreated coconut palm fiber.
[0015] By adopting the technical scheme, the coconut palm fiber is soaked in a NaOH solution, impurities and a small amount of hemicellulose on the surface of the NaOH solution are removed, and the surface of the coconut palm fiber becomes relatively rough and porous. The addition of epoxy resin not only fills the pores on the surface of the coconut palm fiber, but also cross-links with the fiber, enhances the bonding ability with the fiber interface, and thus increases the tensile strength and elongation at break of the coconut palm fiber. The nano-microcrystalline cellulose further improves the interfacial bonding force between the coconut palm fiber and the epoxy resin, improves the skeleton strength of the coconut palm fiber, and further enhances the structural strength and mechanical properties of the coconut palm fiber. Konjac gum, as a binder, increases the bonding between the coconut palm fiber, the epoxy resin and the nano-microcrystalline cellulose, and thus increases the stability of the pretreated coconut palm fiber.
[0016] Preferably, the mass ratio of the coconut palm fiber, epoxy resin and nano-microcrystalline cellulose is 1:0.4-0.8:0.05-0.09.
[0017] By adopting the above technical scheme, the mass ratio of coconut palm fiber, epoxy resin and nano-microcrystalline cellulose is controlled to obtain coconut palm fiber with higher mechanical properties. The coconut palm fiber and epoxy resin are cross-linked to increase the tensile strength and elongation at break of the coconut palm fiber, while the nano-microcrystalline cellulose further improves the interfacial bonding force between the coconut palm fiber and the epoxy resin, improves the skeleton strength of the coconut palm fiber, and further enhances the structural strength and mechanical properties of the coconut palm fiber.
[0018] Preferably, the method for preparing the modified starch comprises the following steps:
[0019] (1) mixing corn starch and sodium chloride solution, stirring at a temperature of 70-80° C. for 30-45 minutes to obtain a mixed solution;
[0020] (2) adding polyvinyl alcohol and epoxidized soybean oil to the mixed solution obtained in step (1) and stirring at a speed of 1000-1500 rpm for 10-20 min to obtain modified starch.
[0021] By adopting the above technical scheme, corn starch is dissolved in a sodium chloride solution, and polyvinyl alcohol and epoxidized soybean oil are added. Polyvinyl alcohol increases the cohesion of the starch slurry and improves the viscosity of the starch slurry. The epoxidized soybean oil has good stability and maintains the stability of the solution system. At the same time, the structural strength and stability of the starch slurry are improved. In the subsequent preparation of the inner packaging film, the compatibility and structural strength of the modified starch mixed with other components are further improved.
[0022] Preferably, the mass ratio of the corn starch, polyvinyl alcohol and epoxidized soybean oil is 1:0.1-0.3:0.02-0.05.
[0023] By adopting the above technical scheme, the mass ratio of corn starch, polyvinyl alcohol and epoxy soybean oil is controlled to obtain modified starch with better structural strength and better structural stability. There is a synergistic effect between corn starch, polyvinyl alcohol and epoxy soybean oil, and polyvinyl alcohol and epoxy soybean oil change the structural stability and strength of corn starch.
[0024] Preferably, the adhesive comprises the following raw materials: xylitol-based multifunctional epoxy resin, dandelion extract, dextrin, cowhide glue, benzoic acid, coupling agent and water.
[0025] By adopting the above technical scheme, xylitol-based multifunctional epoxy resin is used as the base resin, and multiple reaction sites provide the adhesive with a fast reaction speed and a high cross-linking density, thereby ensuring the excellent mechanical properties of the cured product, and being degradable and environmentally friendly. The dandelion extract enables the prepared adhesive to have antibacterial and antimicrobial properties, while enhancing the strength and toughness of the adhesive. The addition of dextrin increases the solubility and viscosity of each component in the system, allowing the components to be better mixed and have strong viscosity. The use of kraft glue as an adhesive further increases the viscosity of the system, and increases the strength and toughness of the adhesive, so that the prepared adhesive is used in subsequent packaging films, and not only has good degradation performance, but also has good viscosity and strength, thereby increasing the mechanical properties of the packaging film.
[0026] Preferably, the preparation method of the dandelion extract comprises the following steps: washing, crushing and sieving the dandelions to obtain dandelion powder, then dispersing the dandelion powder in water and adding cellulase; then adding an ethanol solution with a volume fraction of 70-80% to the dandelion powder, heating and refluxing to obtain an extract, concentrating under reduced pressure to obtain a concentrated solution, adding water to the concentrated solution, and centrifuging and filtering to obtain a dandelion extract.
[0027] By adopting the above technical scheme, dandelion powder is first hydrolyzed with cellulase, which can promote the dissolution of the cell walls in the dandelion particles, degrade the large molecular polysaccharides, proteins and lipids into small molecular substances, and promote the subsequent extraction of dandelion extract. Ethanol is then used for extraction to obtain a dandelion extract with a higher extraction rate.
[0028] Preferably, the plasticizer is tributyl citrate.
[0029] In a second aspect, the present application also provides a method for preparing a degradable packaging film, comprising the following steps:
[0030] A. Preparation of outer layer: polybutylene succinate, polyethylene, polyvinyl alcohol, sodium alginate, coconut palm fiber, plasticizer and nano zinc oxide are mixed and dried;
[0031] B. Preparation of inner layer: mixing modified starch, chitosan, emulsifier, sugarcane fiber, nano titanium dioxide, plasticizer and talcum powder, and drying;
[0032] C. Feed the raw materials of the outer layer and the inner layer into a single screw extruder for plasticizing and co-extrusion at a temperature of 200-260°C to obtain an outer layer film and an inner layer film;
[0033] D. Preparation of adhesive: xylitol-based multifunctional epoxy resin, dandelion extract, dextrin, cowhide glue, benzoic acid, coupling agent and water are mixed, stirred for 2-3 hours, and then coated on one side of the outer film, and then the inner film is attached to the side of the outer film coated with the adhesive, and dried to obtain a degradable packaging film.
[0034] By adopting the above technical scheme, the outer layer, the inner layer and the adhesive are prepared respectively, and finally the outer layer and the inner layer are bonded with the adhesive to obtain a packaging film. The prepared packaging film has good tensile properties and elongation at break, and also has a high degradation rate.
[0035] Preferably, in step A and step B, the drying temperature is 130-140° C., and the drying time is 20-24 h.
[0036] In summary, this application has the following beneficial effects:
[0037] 1. In the present application, both the outer and inner layer raw materials are made of degradable materials, which are environmentally friendly. In addition, among the outer layer raw materials, polybutylene succinate has excellent mechanical properties and heat resistance, and can eventually be degraded into small molecules such as carbon dioxide, water and methane under the action of natural microorganisms. Polyethylene has good transparency, abrasion resistance and impact resistance. Polyvinyl alcohol has good transparency, high tensile strength and good thermal insulation. The mixture of polybutylene succinate, polyethylene and polyvinyl alcohol improves the mechanical properties of the packaging film such as tensile strength, elongation at break and wear resistance.
[0038] 2. In the present application, sodium alginate has good biocompatibility. Sodium alginate is mixed with polyethylene and polyvinyl alcohol to increase the toughness, elongation at break and tensile strength of the packaging film. The outer surface of the coconut palm fiber is rough and porous, presenting a three-dimensional reticular arrangement pattern, has greater elasticity and good wear resistance. Nano zinc oxide is loaded in the pore structure of the coconut palm fiber, which increases the structural strength of the coconut palm fiber and has good ultraviolet resistance and bactericidal properties. Sodium alginate has certain viscosity and is coated on the outer surface of the coconut palm fiber, thereby increasing the adhesion between the nano zinc oxide and the coconut palm fiber, further increasing the structural strength and mechanical properties of the packaging film.
[0039] 3. The inner layer of the present application adopts modified starch, which has good degradability. The modified starch and chitosan are mixed to prepare the film. There are a large number of active hydroxyl groups and amino groups in the chitosan molecules. They have strong chemical reaction ability and strong anion adsorption capacity. They combine with the molecules in the modified starch to form a three-dimensional network structure, which enhances the interaction between the membrane molecular chains and greatly enhances the tensile capacity of the film, so that the prepared film has good mechanical properties. Sugarcane fiber has good antibacterial and toughness. The sugarcane fiber is dispersed in the network structure formed by chitosan and modified starch, which increases the structural strength and toughness of the inner film, thereby improving the mechanical properties of the inner layer. DETAILED DESCRIPTION
[0040] The present application is further described in detail below with reference to the embodiments.
[0041] The raw materials used in the examples and comparative examples can all be obtained from commercial sources, wherein the plasticizer is tributyl citrate.
[0042] Pretreatment of coconut fiber
[0043] Preparation Example 1-1
[0044] The coconut palm fiber is pretreated, comprising the following steps:
[0045] (1) 1 kg of coconut palm fiber is soaked in 10 L of 10% NaOH solution by mass for 30 min, and then rinsed with deionized water to obtain alkali-treated coconut palm fiber;
[0046] (2) the alkali-treated coconut palm fiber obtained in step (1) is mixed with epoxy resin, then nano-microcrystalline cellulose and 0.5 kg of konjac gum are added, stirred at 70 ° C for 2 h, and freeze-dried to obtain pretreated coconut palm fiber, wherein the mass ratio of coconut palm fiber, epoxy resin and nano-microcrystalline cellulose is 1:0.6:0.07.
[0047] Preparation Example 1-2
[0048] The difference from Preparation Example 1-1 is that step (1) is not performed.
[0049] Preparation Example 1-3
[0050] The difference from Preparation Example 1-1 is that in step (2), no epoxy resin is added.
[0051] Preparation Example 1-4
[0052] The difference from Preparation Example 1-1 is that in step (2), no nano-microcrystalline cellulose is added.
[0053] Preparation Example 1-5
[0054] The difference from Preparation Example 1-1 is that the mass ratio of coconut palm fiber, epoxy resin and nano-microcrystalline cellulose is 1:0.4:0.05.
[0055] Preparation Example 1-6
[0056] The difference from Preparation Example 1-1 is that the mass ratio of coconut palm fiber, epoxy resin and nano-microcrystalline cellulose is 1:0.8:0.09.
[0057] Preparation Example 1-7
[0058] The difference from Preparation Example 1-1 is that the mass ratio of coconut palm fiber, epoxy resin and nano-microcrystalline cellulose is 1:1.2:0.12.
[0059] Preparation example of modified starch
[0060] Preparation Example 2-1
[0061] The preparation method of modified starch comprises the following steps:
[0062] (1) 0.5 kg of corn starch and 10 L of 0.3% sodium chloride solution were mixed and stirred at 75° C. for 40 min to obtain a mixed solution;
[0063] (2) adding polyvinyl alcohol and epoxidized soybean oil to the mixed solution obtained in step (1) and stirring at a speed of 1200 rpm for 15 min to obtain modified starch, wherein the mass ratio of corn starch, polyvinyl alcohol and epoxidized soybean oil is 1:0.2:0.035.
[0064] Preparation Example 2-2
[0065] The difference from Preparation Example 2-1 is that in step (2), no polyvinyl alcohol is added.
[0066] Preparation Example 2-2
[0067] The difference from Preparation Example 2-1 is that in step (2), no epoxidized soybean oil is added.
[0068] Preparation Example 2-4
[0069] The difference from Preparation Example 2-1 is that the mass ratio of corn starch, polyvinyl alcohol and epoxidized soybean oil is 1:0.1:0.02.
[0070] Preparation Example 2-5
[0071] The difference from Preparation Example 2-1 is that the mass ratio of corn starch, polyvinyl alcohol and epoxidized soybean oil is 1:0.3:0.05.
[0072] Preparation Example 2-6
[0073] The difference from Preparation Example 2-1 is that the mass ratio of corn starch, polyvinyl alcohol and epoxidized soybean oil is 1:0.5:0.08.
[0074] Example
[0075] Example 1
[0076] A degradable packaging film, comprising an outer layer and an inner layer, wherein the outer layer comprises the following raw materials by weight: 42 kg of polybutylene succinate, 25 kg of polyethylene, 18 kg of polyvinyl alcohol, 7 kg of sodium alginate, 6 kg of coconut palm fiber, 4 kg of plasticizer, and 16 kg of nano zinc oxide;
[0077] The inner layer includes the following raw materials by weight: 25kg of modified starch, 10kg of chitosan, 3kg of emulsifier, 10kg of sugarcane fiber, 2kg of nano titanium dioxide, 4kg of plasticizer, and 14kg of talcum powder; wherein the outer layer and the inner layer are connected by an adhesive.
[0078] The adhesive includes the following raw materials by weight: 60 kg of xylitol-based multifunctional epoxy resin, 8 kg of dandelion extract, 10 kg of dextrin, 2 kg of cowhide glue, 1 kg of benzoic acid, 5 kg of coupling agent, and 80 kg of water.
[0079] The preparation method of dandelion extract comprises the following steps: washing, crushing and passing 1 kg of dandelion through a 30-mesh sieve to obtain dandelion powder, then dispersing 0.8 kg of dandelion powder in 6 L of water, adding 0.16 kg of cellulase, controlling the enzymolysis temperature at 55 DEG C and the enzymolysis time at 80 min; then adding 80 L of 70% ethanol solution by volume to the dandelion powder, heating and refluxing to extract to obtain an extract, concentrating under reduced pressure to obtain a concentrated solution, adding water to the concentrated solution, centrifuging and filtering to obtain the dandelion extract.
[0080] The method for preparing the above-mentioned degradable packaging film comprises the following steps:
[0081] A. Preparation of outer layer: polybutylene succinate, polyethylene, polyvinyl alcohol, sodium alginate, coconut palm fiber, plasticizer and nano zinc oxide are mixed and dried;
[0082] B. Preparation of inner layer: mixing modified starch, chitosan, emulsifier, sugarcane fiber, nano titanium dioxide, plasticizer and talcum powder, and drying;
[0083] C. Feed the raw materials of the outer layer and the inner layer into a single screw extruder for plasticizing and co-extrusion at a temperature of 200-260°C to obtain an outer layer film and an inner layer film;
[0084] D. Preparation of adhesive: xylitol-based multifunctional epoxy resin, dandelion extract, dextrin, cowhide glue, benzoic acid, coupling agent and water are mixed, stirred for 2-3 hours, and then coated on one side of the outer film, and then the inner film is attached to the side of the outer film coated with the adhesive, and dried to obtain a degradable packaging film.
[0085] Wherein, in step A and step B, the drying temperature is 135° C. and the drying time is 22 h.
[0086] The coconut palm fiber was pretreated by using Preparation Example 1-1; and the modified starch was prepared by using Preparation Example 2-1.
[0087] Example 2
[0088] A degradable packaging film, which is different from Example 1 in that the coconut palm fiber is pretreated by using Preparation Example 1-2.
[0089] Example 3
[0090] A degradable packaging film is different from Example 1 in that the coconut palm fiber is pretreated by using Preparation Examples 1-3.
[0091] Example 4
[0092] A degradable packaging film, which is different from Example 1 in that the coconut palm fiber is pretreated by using Preparation Examples 1-4.
[0093] Example 5
[0094] A degradable packaging film is different from Example 1 in that the coconut palm fiber is pretreated by using Preparation Examples 1-5.
[0095] Example 6
[0096] A degradable packaging film is different from Example 1 in that the coconut palm fiber is pretreated using Preparation Examples 1-6.
[0097] Example 7
[0098] A degradable packaging film, which is different from Example 1 in that the coconut palm fiber is pretreated by using Preparation Examples 1-7.
[0099] Example 8
[0100] A degradable packaging film, which is different from Example 1 in that the modified starch is prepared using Preparation Example 2-2.
[0101] Example 9
[0102] A degradable packaging film, which is different from Example 1 in that the modified starch is prepared using Preparation Example 2-3.
[0103] Example 10
[0104] A degradable packaging film, which is different from Example 1 in that the modified starch is prepared using Preparation Examples 2-4.
[0105] Embodiment 11
[0106] A degradable packaging film, which is different from Example 1 in that the modified starch is prepared using Preparation Examples 2-5.
[0107] Example 12
[0108] A degradable packaging film, which is different from Example 1 in that the modified starch is prepared using Preparation Examples 2-6.
[0109] Example 13
[0110] A degradable packaging film, which is different from Example 1 in that the outer layer comprises the following raw materials by weight: 35 kg of polybutylene succinate, 20 kg of polyethylene, 15 kg of polyvinyl alcohol, 5 kg of sodium alginate, 4 kg of coconut palm fiber, 3 kg of plasticizer, and 14 kg of nano zinc oxide;
[0111] The inner layer includes the following raw materials by weight: 20 kg of modified starch, 5 kg of chitosan, 2 kg of emulsifier, 8 kg of sugarcane fiber, 1 kg of nano titanium dioxide, 3 kg of plasticizer, and 12 kg of talcum powder.
[0112] Embodiment 14
[0113] A degradable packaging film, which is different from Example 1 in that the outer layer comprises the following raw materials by weight: 50 kg of polybutylene succinate, 30 kg of polyethylene, 20 kg of polyvinyl alcohol, 9 kg of sodium alginate, 8 kg of coconut palm fiber, 5 kg of plasticizer, and 18 kg of nano zinc oxide;
[0114] The inner layer includes the following raw materials by weight: 30 kg of modified starch, 15 kg of chitosan, 4 kg of emulsifier, 12 kg of sugarcane fiber, 3 kg of nano titanium dioxide, 5 kg of plasticizer, and 16 kg of talcum powder.
[0115] Embodiment 15
[0116] A degradable packaging film, which differs from Example 1 in that no dandelion extract is added to the adhesive.
[0117] Example 16
[0118] A degradable packaging film, which is different from Example 1 in that no dextrin is added to the adhesive.
[0119] Embodiment 17
[0120] A degradable packaging film, which is different from Example 1 in that no cellulase is added in the preparation method of dandelion extract.
[0121] Comparative Example
[0122] Comparative Example 1
[0123] A degradable packaging film, which is different from Example 1 in that the outer layer comprises the following raw materials by weight: 25 kg of polybutylene succinate, 15 kg of polyethylene, 10 kg of polyvinyl alcohol, 3 kg of sodium alginate, 2 kg of coconut palm fiber, 1 kg of plasticizer, and 12 kg of nano zinc oxide;
[0124] The inner layer includes the following raw materials by weight: 15 kg of modified starch, 3 kg of chitosan, 1 kg of emulsifier, 6 kg of sugarcane fiber, 0.5 kg of nano titanium dioxide, 1 kg of plasticizer, and 10 kg of talcum powder.
[0125] Comparative Example 2
[0126] A degradable packaging film, which is different from Example 1 in that the outer layer comprises the following raw materials by weight: 55 kg of polybutylene succinate, 40 kg of polyethylene, 30 kg of polyvinyl alcohol, 12 kg of sodium alginate, 10 kg of coconut palm fiber, 7 kg of plasticizer, and 20 kg of nano zinc oxide;
[0127] The inner layer includes the following raw materials by weight: 35 kg of modified starch, 17 kg of chitosan, 6 kg of emulsifier, 15 kg of sugarcane fiber, 5 kg of nano titanium dioxide, 7 kg of plasticizer, and 18 kg of talcum powder.
[0128] Comparative Example 3
[0129] A degradable packaging film, which is different from Example 1 in that sodium alginate is not added to the outer layer.
[0130] Comparative Example 4
[0131] A degradable packaging film, which is different from Example 1 in that no coconut palm fiber is added to the outer layer.
[0132] Comparative Example 5
[0133] A degradable packaging film, which is different from Example 1 in that nano zinc oxide is not added to the outer layer.
[0134] Comparative Example 6
[0135] A degradable packaging film, which is different from Example 1 in that chitosan is not added to the inner layer.
[0136] Comparative Example 7
[0137] A degradable packaging film, which is different from Example 1 in that sugarcane fiber is not added to the inner layer.
[0138] Performance testing
[0139] The degradable packaging films prepared in the examples and comparative examples were subjected to mechanical property tests.
[0140] Specifically, mechanical property test: according to GB13022-91 test standard, mechanical property test is carried out on a universal testing machine; tear resistance: tested according to ISO34-1 test standard; the test results are shown in Table 1.
[0141] Table 1 Tests of Examples and Comparative Examples
[0142]
[0143]
[0144] As can be seen from Table 1, the degradable packaging films prepared in Examples 1, 5-6, 10-11 and 13-14 of the present application have good mechanical properties and mechanical stability, with an elongation at break of 426%, a tensile strength of 65 MPa, and a tear resistance of 110 MPa.
[0145] In addition, the packaging film prepared in Example 1 was subjected to a degradation performance test: a 10×10 cm 2 Sample pieces of different sizes were buried in the soil at a temperature of 25°C and a soil humidity of 25%. The mass before and after burial in the soil was weighed, and the degradation rate within 3 months was calculated. The test results showed that the degradation rate reached 52% in 1 month, 75% in 2 months, and 99% in 3 months, indicating that the packaging film prepared in this application has obvious improvement in composting degradation rate, and the prepared packaging film has a high decomposition rate and good decomposition effect.
[0146] In the pretreatment of coconut palm fiber in Example 2, NaOH solution is not used to soak the coconut palm fiber. As can be seen from Table 1, compared with Example 1, the prepared packaging film has an elongation at break of 430%, a tensile strength of 60 MPa, and a tear resistance of 105 MPa, and the mechanical properties of the packaging film are slightly decreased, indicating that the NaOH solution makes the surface of the coconut palm fiber rough and porous, which is helpful for the subsequent loading of nano-microcrystalline cellulose, thereby changing the mechanical properties of the subsequent packaging film.
[0147] In Example 3, no epoxy resin is added during the pretreatment of coconut palm fiber, and in Example 4, no nano-microcrystalline cellulose is added during the pretreatment of coconut palm fiber. In Example 7, the mass ratio of coconut palm fiber, epoxy resin and nano-microcrystalline cellulose is changed. As can be seen from Table 1, compared with Example 1, the elongation at break, tensile strength and tear resistance of the packaging films prepared in Examples 3-4 are significantly reduced, while the various properties of the packaging film prepared in Example 7 are worse than those in Example 1, but significantly better than those in Example 3-4, indicating that not adding epoxy resin or nano-microcrystalline cellulose significantly affects the mechanical properties of the subsequent packaging film, and there is a synergistic effect between coconut palm fiber, epoxy resin and nano-microcrystalline cellulose. Coconut palm fiber is cross-linked with epoxy resin, which increases the tensile strength and elongation at break of coconut palm fiber, and nano-microcrystalline cellulose further improves the interfacial bonding force between coconut palm fiber and epoxy resin, improves the skeleton strength of coconut palm fiber, and further enhances the structural strength and mechanical properties of coconut palm fiber.
[0148] In Example 8, no polyvinyl alcohol is added to the modified starch, and in Example 9, no epoxidized soybean oil is added to the modified starch. In Example 12, the mass ratio of corn starch, polyvinyl alcohol and epoxidized soybean oil is changed. As can be seen from Table 1, compared with Example 1, the elongation at break, tensile strength and tear resistance of the packaging films prepared in Examples 8-9 are significantly reduced, while the various properties of the packaging films prepared in Example 12 are worse than those in Example 1, but significantly better than those in Examples 8-9, indicating that not adding polyvinyl alcohol or epoxidized soybean oil affects the properties of the modified starch, and further affects the mechanical properties of the subsequent packaging film. Corn starch, polyvinyl alcohol and epoxidized soybean oil have a synergistic effect. Polyvinyl alcohol and epoxidized soybean oil change the structural stability and strength of corn starch, and have a certain effect on the structural strength of the subsequent packaging film.
[0149] In Example 15, no dandelion extract is added to the adhesive, and in Example 16, no dextrin is added to the adhesive. As can be seen from Table 1, compared with Example 1, the elongation at break, tensile strength and tear resistance of the packaging films prepared in Examples 8-9 are slightly reduced, indicating that the dandelion extract can enhance the strength and toughness of the adhesive, and the addition of dextrin increases the solubility and viscosity of each component in the system, thereby affecting the subsequent mechanical properties of the packaging film.
[0150] In the preparation method of dandelion extract in Example 17, cellulase is not added. As can be seen from Table 1, compared with Example 1, the elongation at break, tensile strength and tear resistance of the prepared packaging film are slightly reduced, indicating that cellulase can promote the dissolution of the cell wall in the dandelion particles, degrade the macromolecular polysaccharides, proteins and lipids into small molecular substances, promote the subsequent extraction of dandelion extract, and obtain dandelion extract with a higher extraction rate, which in turn helps to improve the performance of the subsequent adhesive.
[0151] In Comparative Example 1-2, the component content of the outer layer and the inner layer raw materials was changed. As can be seen from Table 1, compared with Example 1, the elongation at break, tensile strength and tear resistance of the prepared packaging film were significantly reduced, indicating that the component content of the outer layer and the inner layer raw materials is within a certain range, and the prepared packaging film has good mechanical properties.
[0152] No sodium alginate is added to the outer layer of Comparative Example 3, no coconut palm fiber is added to the outer layer of Comparative Example 4, and no nano zinc oxide is added to the outer layer of Comparative Example 5. As can be seen from Table 1, compared with Example 1, the elongation at break, tensile strength and tear resistance of the prepared packaging film are significantly reduced, indicating that sodium alginate can increase the toughness, elongation at break and tensile strength of the packaging film, nano zinc oxide is loaded in the pore structure of the coconut palm fiber, and the structural strength of the coconut palm fiber is increased. Sodium alginate has a certain viscosity and is coated on the outer surface of the coconut palm fiber, thereby increasing the adhesion between nano zinc oxide and the coconut palm fiber, and further increasing the structural strength and mechanical properties of the packaging film.
[0153] In Comparative Example 6, no chitosan is added to the inner layer, and in Comparative Example 7, no sugarcane fiber is added to the inner layer. As can be seen from Table 1, compared with Example 1, the elongation at break, tensile strength and tear resistance of the prepared packaging film are significantly reduced, indicating that chitosan is combined with the molecules in the modified starch to enhance the interaction between the molecular chains of the film. The sugarcane fiber has good toughness. The sugarcane fiber is dispersed in the network structure formed by chitosan and modified starch, which increases the structural strength and toughness of the inner film, thereby improving the mechanical properties of the inner layer.
[0154] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A degradable packaging film, characterized in that: It comprises an outer layer and an inner layer, wherein the outer layer comprises the following raw materials in parts by weight: 35-50 parts of polybutylene succinate, 20-30 parts of polyethylene, 15-20 parts of polyvinyl alcohol, 5-9 parts of sodium alginate, 4-8 parts of coconut palm fiber, 3-5 parts of plasticizer, and 14-18 parts of nano zinc oxide; The inner layer comprises the following raw materials in parts by weight: 20-30 parts of modified starch, 5-15 parts of chitosan, 2-4 parts of emulsifier, 8-12 parts of sugarcane fiber, 1-3 parts of nano titanium dioxide, 3-5 parts of plasticizer, and 12-16 parts of talc; wherein the outer layer and the inner layer are connected by an adhesive; The coconut palm fiber is pre-treated, comprising the following steps: (1) Soaking coconut palm fiber in a NaOH solution, and then washing with deionized water to make it neutral, thereby obtaining alkali-treated coconut palm fiber; (2) mixing the alkali-treated coconut palm fiber obtained in step (1) with epoxy resin, then adding nano-microcrystalline cellulose and konjac gum, stirring at 60-80° C. for 1-2 hours, and freeze-drying to obtain pretreated coconut palm fiber; The mass ratio of the coconut palm fiber, epoxy resin and nano-microcrystalline cellulose is 1:0.4-0.8:0.05-0.09; The preparation method of the modified starch comprises the following steps: (1) Mix corn starch and sodium chloride solution, and stir at a temperature of 70-80°C for 30-45 minutes to obtain a mixed solution; (2) adding polyvinyl alcohol and epoxidized soybean oil to the mixed solution obtained in step (1) and stirring at a speed of 1000-1500 rpm for 10-20 min to obtain modified starch; The mass ratio of the corn starch, polyvinyl alcohol and epoxidized soybean oil is 1:0.1-0.3:0.02-0.
05.
2. A degradable packaging film according to claim 1, characterized in that: The adhesive comprises the following raw materials: xylitol-based multifunctional epoxy resin, dandelion extract, dextrin, cowhide glue, benzoic acid, coupling agent and water.
3. A degradable packaging film according to claim 2, characterized in that: The preparation method of the dandelion extract comprises the following steps: washing, crushing and sieving dandelions to obtain dandelion powder, then dispersing the dandelion powder in water and adding cellulase; then adding an ethanol solution with a volume fraction of 70-80% to the dandelion powder, heating and refluxing to obtain an extract, concentrating under reduced pressure to obtain a concentrated solution, adding water to the concentrated solution, centrifuging and filtering to obtain the dandelion extract.
4. The degradable packaging film according to claim 1, characterized in that: The plasticizer is tributyl citrate.
5. The method for preparing a degradable packaging film according to any one of claims 1 to 4, characterized in that: The following steps are involved: A. Preparation of outer layer: polybutylene succinate, polyethylene, polyvinyl alcohol, sodium alginate, coconut palm fiber, plasticizer and nano zinc oxide are mixed and dried; B. Preparation of inner layer: mixing modified starch, chitosan, emulsifier, sugarcane fiber, nano titanium dioxide, plasticizer and talcum powder, and drying; C. Feed the raw materials of the outer layer and the inner layer into a single screw extruder for plasticizing and co-extrusion at a temperature of 200-260°C to obtain an outer layer film and an inner layer film; D. Preparation of adhesive: xylitol-based multifunctional epoxy resin, dandelion extract, dextrin, cowhide glue, benzoic acid, coupling agent and water are mixed, stirred for 2-3 hours, and then coated on one side of the outer film, and then the inner film is attached to the side of the outer film coated with the adhesive, and dried to obtain a degradable packaging film.