A method for preparing a graphene-loaded electrode using CO2 reduction product as a carbon source

By using CO2 reduction products as carbon sources, combined with electrospinning and electrocatalytic reduction technology, graphene-loaded electrodes are prepared, which solves the problem of unenvironmental use of carbon sources and hydrogen, and achieves efficient and environmentally friendly graphene preparation, suitable for liquid flow Battery, improves the power density of the battery.

CN116119644BActive Publication Date: 2024-11-15SHAANXI YUNENG GRP ENERGY & CHEM RES INST CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211658236.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-11-15
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

In the existing graphene preparation methods, the use of carbon source and hydrogen is not environmentally friendly, and the products produced during electrocatalytic reduction of CO2 need to be separated and purified, which is inconvenient to use.

Method used

The graphene-loaded electrode is prepared by combining electrospinning and electrocatalytic reduction by using CO2 reduction products as carbon source, which avoids the contradiction between carbon products and hydrogen, saves energy and is environmentally friendly, and is morphologically controlled by controlling the amount of carbon products and hydrogen. Graphene.

Benefits of technology

It realizes environmentally friendly graphene preparation, reduces the use and processing steps of raw materials, improves the structural and morphological diversity of graphene, is suitable for liquid flow batteries, and increases the power density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116119644B_ABST
    Figure CN116119644B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of graphene preparation, and relates to a method for preparing a graphene-loaded electrode using a CO2 reduction product as a carbon source, comprising the following steps: 1) adding polyacrylonitrile to N, N-2 methylamide to obtain a precursor solution; 2) the precursor solution is electrostatically spun to obtain a spinning membrane; 3) the spinning membrane is carbonized to form a carbon-based material under the action of a protective gas; 4) the CO2 gas source is electrocatalytically reduced to obtain a gaseous product mixed with hydrocarbon gas and hydrogen, and the gaseous product is passed into a tubular furnace containing a carbon-based material, and calcined, cooled, washed, and dried in sequence to obtain a graphene-loaded carbon material electrode. The graphene-loaded electrode preparation method proposed by the present invention avoids the contradiction between carbon products and hydrogen in the CO2 reduction process, and the graphene morphology is controllable. At the same time, the method does not require additional hydrogen, is energy-saving and environmentally friendly, and meets the dual carbon goals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of graphene preparation, and relates to a method for preparing a graphene-loaded electrode using a CO2 reduction product as a carbon source. Background Art

[0002] With the gradual development of society, the widespread use of renewable energy has become a general trend. However, the unstable and discontinuous characteristics of renewable energy limit its use. Therefore, flow batteries, as an energy storage technology, have good application prospects in solving the problems of renewable energy. At present, carbon-based materials are used as electrodes for flow batteries, but the original carbon electrodes usually cannot meet people's power requirements for flow batteries.

[0003] As a carbon material with high electron mobility and ultra-high specific surface area, graphene is given high expectations in electrode modification. Therefore, in order to improve the power of liquid flow batteries, many studies have been conducted on the loading of graphene materials, usually by electrodeposition or chemical deposition on graphite felt or carbon felt materials to form graphene, or by using a hydrothermal method to load the prepared graphene powder on the electrode substrate. Chemical vapor deposition is one of the common methods for preparing graphene on electrodes. The gas sources used are mainly carbon sources and hydrogen. The defects of this method are: it is not environmentally friendly and there is a problem between the production of hydrogen and carbon by the carbon source in electrochemical deposition. As one of the atmospheric pollutants, CO2 is one of the atmospheric pollutants. In order to achieve the purpose of CO2 reuse and environmental protection, the existing method is to use electrocatalytic reduction of CO2. During the electrocatalytic reduction reaction, due to the different working electrodes, gas products including methane, formic acid, ethylene, ethanol and hydrogen will appear. When these products are reused, various carbon products and hydrogen need to be separated and purified, which is inconvenient to use. Summary of the invention

[0004] The purpose of the present invention is to propose a method for preparing a graphene-loaded electrode using CO2 reduction products as a carbon source. This method avoids the contradiction between carbon products and hydrogen during the CO2 reduction process, and the graphene morphology is controllable. At the same time, this method does not require additional hydrogen, is energy-saving and environmentally friendly, and meets the dual carbon goals.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for preparing a graphene-loaded electrode using a CO2 reduction product as a carbon source comprises the following steps:

[0007] 1) adding polyacrylonitrile to N,N-dimethylformamide to obtain a precursor solution;

[0008] 2) The precursor solution of step 1) is subjected to electrospinning to obtain a spinning membrane;

[0009] 3) The spinning membrane of step 2) is carbonized under the action of protective gas to form a carbon-based material;

[0010] 4) electrocatalytically reducing the CO2 gas source to obtain a gaseous product of a mixture of hydrocarbon gas and hydrogen, and passing the gaseous product into a tubular furnace containing the carbon material of step 3), and sequentially calcining, cooling, washing, and drying to obtain a graphene-loaded carbon material electrode.

[0011] Furthermore, in the step 1), the mass concentration of polyacrylonitrile in the precursor liquid is 5% to 15%.

[0012] Furthermore, in the step 2), the thickness of the spinning membrane is 0.015 mm to 1.0 mm, and the size is 3 cm×3 cm to 15 cm×15 cm.

[0013] Furthermore, in the step 3), the protective gas is nitrogen or argon, the carbonization temperature is 400° C. to 800° C., the heating rate is 2° C. / min, and the carbonization time is 1 h to 4 h.

[0014] Furthermore, in the step 4), the working electrode used for electrocatalytic reduction is a metal-based electrode; and the volume ratio of the hydrocarbon gas to hydrogen is 1:5-20.

[0015] Furthermore, the metal-based electrode is a Cu-based electrode, a Sn-based electrode, a Fe-based electrode, a Ni-based electrode, a Co-based electrode or a Mn-based electrode.

[0016] Furthermore, in the step 4), the gaseous product introduction rate is 80 sccm to 150 sccm; the calcination temperature is 800° C. to 1200° C., and the calcination time is 3 h to 12 h.

[0017] A graphene-loaded carbon material electrode prepared by a method for preparing a graphene-loaded electrode using a CO2 reduction product as a carbon source.

[0018] An application of the graphene-loaded carbon material electrode in a liquid flow battery.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The method of the present invention prepares graphene, and the gas source used is the product of catalytic reduction of CO2, which is more environmentally friendly than directly using carbon source and hydrogen.

[0021] 2. The CO2 catalytic reduction reaction used in the method of the present invention, in which the hydrogen produced by the side reaction is also one of the raw materials required subsequently, avoids the problem between hydrogen production and carbon production in the electrocatalytic reduction of CO2, and saves raw materials.

[0022] 3. The method of the present invention provides a new application method of CO2 reduction products, combining CO2 reduction and graphene preparation, and producing graphene with different structures and morphologies by controlling the amount of carbon products and hydrogen.

[0023] 4. The method of the present invention selects a metal-based electrode as a working electrode, controls the amount of carbon products and hydrogen, and directly uses the CO2 reduction product for the preparation of graphene. There is no need to separate the CO2 reduction product, so it is easy to use and reduces the processing steps and utilization costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Flow chart for preparing graphene-loaded carbon electrodes;

[0025] Figure 2 This is an electron microscope image of the electrode prepared in Example 1;

[0026] Figure 3 This is an electron microscope image of the electrode prepared in Example 2;

[0027] Figure 4 This is an electron microscope image of the electrode prepared in Example 3;

[0028] Figure 5 This is the TEM image of the electrode prepared in Example 1. DETAILED DESCRIPTION

[0029] The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0030] The object of the present invention is to provide a method for preparing a graphene-loaded electrode using a CO2 reduction product as a carbon source.

[0031] See also Figure 1 The preparation method provided by the present invention comprises the following steps.

[0032] Step 1), polyacrylonitrile (PAN) and a solvent are mixed to obtain a PAN solution, which is used as an electrospinning precursor solution.

[0033] Step 2), electrospinning the precursor solution of step 1) to form a spinning membrane with a certain area and thickness.

[0034] Step 3), carbonizing the spinning membrane obtained in step 2) at a certain temperature under the action of a protective gas to form a carbon-based material.

[0035] In step 4), the CO2 gas source is electrocatalytically reduced to obtain a gaseous product of a mixture of hydrocarbon gas and hydrogen, and the gaseous product is introduced into a tubular furnace containing the carbon material of step 3), and sequentially calcined, cooled, washed, and dried to obtain a graphene-loaded carbon material electrode.

[0036] In step 1) of the present invention, the solvent in the PAN solution is N,N-dimethylformamide DMF or dimethylacetamide DMAc, and the mass concentration of PAN in the PAN solution is 5% to 15%.

[0037] In step 2) of the present invention, the thickness of the spinning membrane is 0.015 mm to 1.0 mm, and the size is 3 cm×3 cm to 15 mm×15 cm.

[0038] In step 3) of the present invention, the protective gas is an inert gas, specifically nitrogen or argon. The carbonization temperature is 400° C. to 800° C., the heating rate is 2° C. / min, and the carbonization time is 1 h to 4 h.

[0039] In step 4) of the present invention, the working electrode used in the electrocatalytic reduction is a metal-based electrode; the metal-based electrode is a Cu-based electrode, a Sn-based electrode, a Fe-based electrode, a Ni-based electrode, a Co-based electrode or a Mn-based electrode. The metal-based electrode used in this embodiment can be a simple metal electrode or a composite metal electrode. During the electrocatalytic reduction, the other electrode is a carbon rod.

[0040] In step 4) of the present invention, the gaseous product is divided into hydrocarbon gas and hydrogen, and the volume ratio of hydrocarbon gas to hydrogen is 1:5-20; the calcination temperature is 800°C-1200°C, and the calcination time is 3h-12h.

[0041] The hydrocarbon gases (ie, carbon products) in the present invention include, but are not limited to, methane and ethylene.

[0042] The graphene-loaded carbon material electrode prepared by the present invention can be used as a carbon-based electrode with high specific surface area and high electrical conductivity in the field of liquid flow batteries.

[0043] Example 1

[0044] 1) Weigh 0.8 g of polyacrylonitrile and dissolve it in 10 g of N,N-2-methylamide. Stir evenly at room temperature to prepare an electrospinning solution with a concentration of 8%.

[0045] 2) The electrospinning solution was electrospun to obtain a spinning membrane with a size of 5 cm×12 cm and a thickness of 0.15 mm.

[0046] 3) The spun membrane was placed in a tubular furnace for carbonization at a carbonization temperature of 500°C for 2 hours at a heating rate of 2°C / min. After cooling to room temperature, the membrane was taken out to obtain a PAN-based carbon material.

[0047] 4) Using a plasma-treated polycrystalline Cu-based electrode as a working electrode and a carbon rod as the other electrode, electrocatalytic reduction of CO2 was performed to obtain hydrocarbon products and hydrogen, with a volume ratio of hydrocarbon gas to hydrogen of 1:5; the gaseous product was introduced into a tubular furnace containing a PAN-based carbon material at a rate of 80 sccm, and the reaction was carried out at a temperature of 1100°C for 6 hours; after the reaction, the product was cooled to room temperature, taken out, washed with water, and dried to obtain a graphene-loaded carbon electrode.

[0048] The graphene-loaded carbon electrode prepared in this example was subjected to electron microscopy scanning to obtain a SEM morphology image (see Figure 2 ).

[0049] Furthermore, the graphene-loaded carbon electrode was scanned by transmission electron microscopy to obtain a TEM image (see Figure 5 ).

[0050] Example 2

[0051] (1) Weigh 1.0 g of polyacrylonitrile and dissolve it in 10 g of N,N-2-methylamide. Stir evenly at room temperature to prepare an electrospinning solution with a concentration of 10%.

[0052] (2) The electrospinning solution of step 1) was electrospun to obtain a spinning membrane with a size of 5 cm×12 cm and a thickness of 0.05 mm.

[0053] (3) The spun membrane of step 2) is placed in a tubular furnace for carbonization at a carbonization temperature of 500°C for 2 hours at a heating rate of 2°C / min. After cooling to room temperature, the membrane is taken out to obtain a PAN-based carbon material.

[0054] (4) A Cu-based electrode containing Cu2O was used as the working electrode and the other electrode was a carbon rod. CO2 was electrocatalytically reduced to obtain hydrocarbon products and hydrogen. The volume ratio of hydrocarbon gas to hydrogen was 1:10. The gaseous product was introduced into a tubular furnace containing PAN-based carbon material at a rate of 100 sccm at a temperature of 900°C for 4 hours. After the reaction, the mixture was cooled to room temperature, taken out, washed with water, and dried to obtain a graphene-loaded carbon electrode.

[0055] The graphene-loaded carbon electrode prepared in this example was subjected to electron microscopy scanning to obtain a SEM morphology image (see Figure 3 ).

[0056] Example 3

[0057] (1) Weigh 1.2 g of polyacrylonitrile and dissolve it in 10 g of N,N-methylamide. Stir it evenly at room temperature to prepare an electrospinning solution with a concentration of 12%.

[0058] (2) The electrospinning solution of step 1) was electrospun to obtain a spinning membrane with a size of 5 cm×5 cm and a thickness of 0.12 mm.

[0059] (3) The spun membrane is placed in a tubular furnace for carbonization at a temperature of 400°C for 2 hours. After cooling to room temperature, the membrane is taken out to obtain a PAN-based carbon material.

[0060] (4) A Cu-based electrode formed by a Cu-Zn nanocomposite material was used as a working electrode, and the other electrode was a carbon rod. CO2 was electrocatalytically reduced to obtain hydrocarbon products and hydrogen, and the volume ratio of hydrocarbon gas to hydrogen was 1:20. The gaseous product was introduced into a tubular furnace containing a PAN-based carbon material at a rate of 150 sccm at a temperature of 800°C for 4 hours. After the reaction was completed, the mixture was cooled to room temperature, taken out, washed with water, and dried to obtain a graphene-loaded carbon electrode.

[0061] The graphene-loaded carbon electrode prepared in this example was subjected to electron microscopy scanning to obtain a SEM morphology image (see Figure 4 ).

[0062] Example 4

[0063] (1) Weigh 1.4 g of polyacrylonitrile and dissolve it in 10 g of N,N-methylamide. Stir it evenly at room temperature to prepare an electrospinning solution with a concentration of 14%.

[0064] (2) The electrospinning solution of step 1) is electrospun to obtain a spinning membrane with a size of 10 cm×10 cm and a thickness of 0.05 mm.

[0065] (3) The spun membrane was placed in a tubular furnace for carbonization at a temperature of 400°C for 2 hours. After cooling to room temperature, the membrane was taken out to obtain a PAN-based carbon material.

[0066] (4) A Cu-based electrode formed of a nano Cu-Pt composite material is used as a working electrode, and the other electrode is a carbon rod. CO2 is electrocatalytically reduced to obtain hydrocarbon products and hydrogen, and the volume ratio of hydrocarbon gas to hydrogen is 3:20. The gaseous product is passed into a tubular furnace containing PAN-based carbon material at 100 sccm, at a temperature of 800°C, and reacted for 6 hours. After the reaction, it is cooled to room temperature, taken out, washed with water, and dried; a graphene-loaded carbon electrode is obtained.

[0067] Comparative Example

[0068] Using the impregnation method, 0.1 mg of graphene powder was ultrasonically dispersed in 10 mL of nafion solution to obtain a mixed dispersion. The carbon felt (denoted as CF) and the electrospun carbon felt after carbonization in Example 1 (denoted as ECF) were immersed in the mixed dispersion, ultrasonically treated for 5 minutes, and dried at 80°C. The obtained products were respectively denoted as GO-CF and GO-ECF.

[0069] At the same time, the graphene carbon electrode (denoted as GO-C-ECF) prepared in Example 1.

[0070] The above three electrode products were subjected to BET test. The BET test results showed that the specific surface areas of the three different electrodes were GO-C-ECF>GO-ECF>GO-CF, and the specific surface area of ​​CF was smaller than that of GO-CF; the specific surface area of ​​GO-C-ECF was 315.3m 2 ·g -1 , which is 100 times higher than carbon felt CF.

[0071] Taking the all-vanadium flow battery as an example, the above-mentioned groups of carbon electrodes were used as the positive electrode of the all-vanadium flow battery for CV testing. The results showed that the -Ipa / Ipc of GO-C-ECF was closer to 1, that is, it had better electrochemical reversibility. Using GO-C-ECF as the positive and negative electrodes of the all-vanadium flow battery at a current density of 150mA·cm -2 In this case, it still has an energy efficiency of 73.6%, which is about 11% higher than the original carbon felt electrode.

[0072] The present invention combines electrospinning, electrocatalytic reduction of CO2 and vapor deposition, and directly prepares graphene using the CO2 reduction product, which is energy-saving and environmentally friendly. The content of carbon products and hydrogen is controlled by the working electrode to produce graphene-loaded electrodes with different morphologies. The prepared graphene-loaded carbon electrode is a carbon electrode with high specific surface area and high electrical conductivity, which can improve the battery power density and is applied to the field of liquid flow batteries to provide more reaction sites for electrode reactions.

Claims

1. A CO 2 Method for preparing graphene-loaded electrode with reduction product as carbon source, It is characterized in that The following steps are involved: 1) adding polyacrylonitrile to N,N-dimethylformamide to obtain a precursor solution; 2) The precursor solution of step 1) is subjected to electrospinning to obtain a spinning membrane; 3) The spinning membrane of step 2) is carbonized under the action of protective gas to form a carbon-based material; 4) CO 2 The gas source is electrocatalytically reduced to obtain a gaseous product of a mixture of hydrocarbon gas and hydrogen, and the gaseous product is introduced into a tubular furnace containing the carbon material of step 3), and is sequentially calcined, cooled, washed, and dried to obtain a graphene-loaded carbon material electrode; in the step 4), the working electrode used for the electrocatalytic reduction is a metal-based electrode; the volume ratio of the hydrocarbon gas to hydrogen is 1:5-20; the metal-based electrode is a Cu-based electrode, a Sn-based electrode, a Fe-based electrode, a Ni-based electrode, a Co-based electrode, or a Mn-based electrode.

2. The method according to claim 1 2 Method for preparing graphene-loaded electrode with reduction product as carbon source, It is characterized in that In the step 1), the mass concentration of polyacrylonitrile in the precursor liquid is 5% to 15%.

3. The method according to claim 2 2 Method for preparing graphene-loaded electrode with reduction product as carbon source, It is characterized in that In the step 2), the thickness of the spinning membrane is 0.015 mm to 1.0 mm, and the size is 3 cm×3 cm to 15 cm×15 cm.

4. The method according to claim 3 2 Method for preparing graphene-loaded electrode with reduction product as carbon source, It is characterized in that In the step 3), the protective gas is nitrogen or argon, the carbonization temperature is 400° C. to 800° C., the heating rate is 2° C. / min, and the carbonization time is 1 h to 4 h.

5. The method according to claim 4 2 Method for preparing graphene-loaded electrode with reduction product as carbon source, It is characterized in that In the step 4), the gas product introduction rate is 80 sccm to 150 sccm; the calcination temperature is 800° C. to 1200° C., and the calcination time is 3 h to 12 h.

6. A method according to claim 1 using CO 2 A graphene-loaded carbon material electrode prepared by a method for preparing a graphene-loaded electrode with a reduction product as a carbon source.

7. Use of the graphene-supported carbon material electrode as claimed in claim 6 in a liquid flow battery.