A kind of cable semi-conductive shielding material of ionic liquid modified conductive carbon black and preparation method thereof

CN116120655BActive Publication Date: 2024-11-26GUANGDONG POWER GRID CO LTD DONGGUAN POWER SUPPLY BUREAU +1
View PDF 0 Cites -1 Cited by

Patent Information

Application Number
CN202211076880.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-02
Publication Date
2024-11-26
Estimated Expiration
2042-09-02

AI Technical Summary

Technical Problem

Conductive carbon black in existing high-voltage cable semiconductors is prone to agglomeration, which makes it difficult for electrical and mechanical properties to meet the requirements at the same time, and the agglomerates form protrusions to cause insulation failure.

Method used

Using ionic liquid as the dispersant of conductive carbon black, the dispersion of conductive carbon black in the matrix resin is improved through non-covalent bond modification technology, and the high-dispersible conductive carbon black filler is prepared by ultrasonic dispersion and other methods during the preparation process. , combining high-speed mixing and twin-screw extrusion technology to prepare semiconductor semiconductors for high-voltage cables.

Benefits of technology

It significantly improves the uniform dispersion stability of conductive carbon black in the matrix resin, reduces agglomeration phenomenon, improves the surface finish and performance of high-voltage cable semiconductor, and has excellent resistivity, mechanical properties and thermal properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003830275030000051
    Figure BDA0003830275030000051
Patent Text Reader

Abstract

The present invention provides a cable semi-conductive shielding material of ionic liquid modified conductive carbon black and a preparation method thereof. The semi-conductive shielding material composition comprises a substrate, conductive carbon black, ionic liquid, lubricant, antioxidant, and cross-linking agent. According to their weight parts, the substrate is 58-64 parts, the conductive carbon black is 27-34 parts, the ionic liquid is 1-5 parts, the lubricant is 1-2 parts, the antioxidant is 0.3-0.7 parts, and the cross-linking agent is 0.4-2.2 parts. The present invention also provides a preparation method of ionic liquid modified conductive carbon black. When the conductive carbon black treated by the method is used for ultra-smooth high-voltage cable semi-conductive inner shielding material, the shielding material has relatively excellent electrical properties and mechanical properties, thereby solving the problem that the conductive carbon black is easy to agglomerate during the extrusion process of the semi-conductive shielding material in the existing preparation method, making it difficult for the extruded surface finish to meet the ultra-smooth requirements, and solving the problems of rough surface and poor surface finish of the shielding material caused by the friction between the matrix resin and the equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of cross-linked polyethylene cable materials, and in particular relates to a cable semi-conductive shielding material of ionic liquid modified conductive carbon black and a preparation method thereof. Background Art

[0002] In recent years, with the upgrading and construction of large-scale projects such as power grid transformation and ultra-high voltage, the demand for high-voltage cables has increased rapidly. XLPE (Cross linked polyethylene) extruded insulated cable has been widely used in high-voltage cables because of its simple process, large transmission capacity, easy maintenance and low cost. The semi-conductive shielding layer is an important part of the XLPE cable structure. It has the function of improving the electric field distribution and eliminating the air gap at the interface between the conductor and the insulation layer, avoiding insulation failure due to local discharge. The raw material used for the semi-conductive shielding layer is a semi-conductive shielding material, which is generally obtained by melt blending and compounding the base resin, conductive carbon black and processing aids.

[0003] Since conductive carbon black itself has a relatively large specific surface area and high surface energy, it is easy to agglomerate, so its dispersion in the matrix resin is hindered. In addition, these conductive carbon black agglomerates will form burrs or protrusions during the extrusion of the shielding material, causing local stress concentration in the cable insulation layer, making it more vulnerable to damage and reducing the service life of the cable. In order to make the dispersion performance of conductive carbon black in the matrix resin better, so as to play a greater advantage in polymer materials, the modification of conductive carbon black has become a more important issue nowadays.

[0004] Ionic liquids are liquid ionic compounds composed of organic cations and organic (or inorganic) anions. They are also called room temperature molten salts and have a relatively low melting temperature. At the same time, ionic liquids themselves have relatively excellent properties: non-volatile, non-flammable, good thermal stability, wide liquid temperature range, high conductivity, strong solubility and other excellent properties. Conductive carbon black and ionic liquids can interact with each other, and ionic liquids adhere to conductive carbon black. At the same time, when conductive carbon black is filled into composite materials, ionic liquids can also play their own advantages and modify the multi-component synergistic effect of high-voltage cable semi-conductive shielding materials.

[0005] Prior art document 1 (CN111117051A) discloses an inner shielding material for cables with anti-copper damage function and a preparation method thereof. The shielding material comprises the following components by weight: EVA, 30 to 35 parts; white oil, 5 to 8 parts; dispersant, 0.5 to 4 parts; cross-linking agent, 0.5 to 3 parts; plasticizer, 10 to 12 parts; ionic liquid surfactant, 0.6-0.8 parts; conductive carbon black, 30 to 32 parts; antioxidant, 0.1 to 0.5 parts; anti-adhesive agent, 12 to 18 parts.

[0006] Prior art document 2 (CN106750848A) discloses an easy-to-peel semi-conductive shielding material, which is prepared from the following raw materials by weight: 40-45 parts of EVA, 32-38 parts of conductive carbon black, 5-8 parts of white oil, 2-5 parts of lubricant, 0.5-4 parts of dispersant, 0.1-0.5 parts of antioxidant, 0.5-3 parts of cross-linking agent, 12-18 parts of anti-adhesive agent, and 0.6-0.8 parts of trisiloxane imidazolium ionic liquid surfactant. The melt index of ethylene vinyl acetate copolymer is 5.5-6.3g / 10min, the softening point is less than 40°C, the mass percentage of total vinyl acetate in the polymer is 25-35%, the anti-adhesive agent is nitrile rubber, and the ionic liquid surfactant is trisiloxane imidazolium ionic liquid surfactant.

[0007] In the above two prior art documents, the role of adding a very small amount of ionic liquid is to use its lipophilic group to reduce the interfacial tension of white oil and improve the wettability of white oil and EVA, and there is no impact on the dispersion of conductive carbon black and the conductive network of the entire material system. The difference between this scheme and the comparative document is that in the preparation method, ionic liquid is used as a conductive carbon black dispersant to improve the dispersibility of conductive carbon black in the matrix resin, and at the same time, the inherent conductivity of the ionic liquid is used to help form a more stable connected conductive network in the base resin, so as to achieve the preparation of a high-voltage cable semi-conductive shielding material with high resistivity stability and ultra-smooth surface. Summary of the invention

[0008] The purpose of the present invention is to overcome the problem that conductive carbon black is easily agglomerated during the extrusion process of high-voltage cable semi-conductive shielding materials in the prior art, making it difficult for the electrical and mechanical properties of the shielding material to meet the requirements at the same time. In addition, these agglomerates will form protrusions, causing local electric field concentration in the insulating layer, thereby causing insulation failure. A cable semi-conductive shielding material of ionic liquid modified conductive carbon black and a preparation method thereof are provided.

[0009] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0010] The present invention discloses a semi-conductive shielding material for cables of ionic liquid-modified conductive carbon black, comprising a substrate, conductive carbon black, a cross-linking agent, an antioxidant, a lubricant, an ionic liquid, and a lubricant; the characteristics are that the weight proportions of the components are as follows:

[0011] 58-64 parts of base material, 27-35 parts of conductive carbon black, 1-5 parts of ionic liquid, 1-2 parts of lubricant, 0.3-0.7 parts of antioxidant, and 0.4-2.2 parts of crosslinking agent.

[0012] Preferably, the substrate is one or more of ethylene-butyl acrylate or ethylene-ethyl acrylate, and the substrate performance is regulated according to the content of the second copolymerized monomer, and the mass ratio of the second copolymerized monomer in the substrate is controlled to be between 16 and 20%.

[0013] Preferably, the conductive carbon black is a high-purity conductive carbon black, with a DBP absorption value of 150-170 ml / 100 g, an ash content of <0.2%, a 325-mesh sieve residue content of <8 ppm, and does not contain any excess impurities.

[0014] Preferably, the cross-linking agent is one or more of diisopropylbenzene peroxide and dicumyl peroxide.

[0015] Preferably, the ionic liquid is an imidazolium ionic liquid.

[0016] Preferably, the lubricant is one or more of zinc stearate and pentaerythritol.

[0017] Preferably, the antioxidant is one or more of the antioxidant 1010 and the antioxidant 300 .

[0018] The present invention also discloses a method for preparing highly dispersible conductive carbon black, characterized in that the preparation method comprises the following steps:

[0019] Step 1, removing moisture from the conductive carbon black according to the weight ratio, setting the oven temperature to 100° C. to 120° C., and drying for 4 to 5 hours;

[0020] Step 2, take 300-400 ml of deionized water in a beaker, add the ionic liquid into the deionized water according to the weight ratio, and stir evenly with a magnetic stirrer at a speed of 70-100 rpm for 10-15 minutes;

[0021] Step 3, slowly pour the conductive carbon black in step 1 into the dispersion obtained in step 2 according to the weight ratio, stir for 30 minutes, and then let it stand for a period of time, the standing time is 15 minutes;

[0022] Step 4, after the stirring is completed, ultrasonically disperse the mixed solution of the ionic liquid and the conductive carbon black in an ultrasonic disperser for 1 to 2 hours to obtain a dispersed suspension of the ionic liquid modified conductive carbon black;

[0023] Step 5, putting the dispersed suspension of conductive carbon black in step 4 into an oven for drying to obtain a highly dispersed conductive carbon black filler, the oven temperature is 110° C. to 130° C., and the drying time is 12 h to 24 h.

[0024] The present invention also discloses a method for preparing a semi-conductive shielding material for a cable, wherein the method comprises the following steps:

[0025] Step a, mixing the highly dispersible conductive carbon black filler and the remaining processing aids in a high-speed mixer according to the weight ratio, and then adding the base material of the set weight ratio and mixing at 45-50° C., wherein the high-speed mixer is controlled at a speed between 150-250 rpm;

[0026] Step b, melt-extrude the mixture obtained in step a in a twin-screw extruder at an extrusion temperature of 180° C. and a main engine speed of 120 rpm, and then pelletize and dry to obtain a granular material;

[0027] Step c, putting the dried granular material obtained in step b into a container, placing it in an oven at 65°C to heat the granular material to 65°C, then mixing the granular material with a cross-linking agent of a set weight ratio that is evenly ground, and then placing it in an oven at 65°C for 10 hours to allow the granular material to fully absorb the cross-linking agent, thereby obtaining a high-voltage cable semi-conductive shielding material.

[0028] The beneficial effects of the present invention are:

[0029] The conductive carbon black is modified by non-covalent bonds using imidazole ionic liquids. Compared with covalent modification, non-covalent modification retains the good surface structure of the conductive carbon black, so that its excellent electrical properties, mechanical properties, and thermal properties can be better exerted. When the ionic liquid is used for the non-covalent modification of the conductive carbon black, the hydrophobic part is wrapped on the conductive carbon black through van der Waals forces and non-covalent interactions such as π-π, and the hydrophilic part is directly combined with the polar end of the matrix, thereby enhancing the dispersibility. These non-covalent modifications increase the dispersion uniformity and stability of the conductive carbon black in the matrix resin. When the conductive carbon black produced by the present invention is used for the semi-conductive shielding material of the high-voltage cable, the agglomeration phenomenon of the conductive carbon black in the matrix resin is reduced, and the surface finish of the semi-conductive shielding material of the high-voltage cable is improved. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the scheme of the present invention, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work should fall within the scope of protection of the present invention.

[0031] Example 1

[0032] As an embodiment of the present invention, a semi-conductive shielding material for high-voltage cross-linked polyethylene cable and a preparation method thereof are provided. The semi-conductive shielding material for high-voltage cables comprises, by weight, 61.25 parts of a base material, 35 parts of conductive carbon black, 1 part of an ionic liquid, 1 part of a lubricant, 0.5 parts of an antioxidant, and 0.75 parts of a cross-linking agent.

[0033] The substrate is EEA resin with an EA content of 17 wt %. The melt index at 190° C. and 2.16 kg is 8.5 g / min, and the elongation at break is 900%.

[0034] The conductive carbon black is a high-purity conductive carbon black with a DBP absorption value of 158 ml / 100 g, an ash content of 0.2%, a 325-mesh sieve residue content of 5 ppm, and does not contain impurity elements such as sulfur and silicon.

[0035] The ionic liquid shown is 1-butyl-3-ethylimidazolium chloride ([Emim]Cl).

[0036] The lubricant is a compound of zinc stearate and pentaerythritol, with a mass ratio of 1:1.

[0037] The antioxidant is a mixture of antioxidant 1010 and antioxidant 300, with a mass ratio of 1:1.

[0038] The crosslinking agent is diisopropylbenzene peroxide (BIPB).

[0039] This embodiment adopts a preparation method of highly dispersible conductive carbon black filler, characterized in that the preparation method comprises the following steps:

[0040] (1) removing moisture from the conductive carbon black according to the weight ratio, setting the oven temperature to 110° C., and drying for 4 hours;

[0041] (2) Take 400 ml of deionized water in a beaker, add the ionic liquid into the deionized water according to the weight ratio, and stir evenly using a magnetic stirrer at a speed of 80 rpm for 15 min;

[0042] (3) slowly pouring the conductive carbon black in step 1 into the dispersion obtained in step 2 according to the weight ratio, stirring for 30 minutes, and then standing for a period of time, the standing time is 15 minutes;

[0043] (4) After the stirring is completed, the mixed solution of the ionic liquid and the conductive carbon black is ultrasonically dispersed in an ultrasonic disperser for 2 hours to obtain a dispersed suspension of the ionic liquid modified conductive carbon black;

[0044] (5) The dispersed suspension of conductive carbon black in step 4 is placed in an oven for drying to obtain a highly dispersed conductive carbon black filler. The oven temperature is 110° C. and the drying time is 12 h.

[0045] The method for preparing the semi-conductive shielding material for high-voltage cables of this embodiment comprises the following steps:

[0046] (1) uniformly mixing a highly dispersible conductive carbon black filler and a coupling agent in a weight ratio to perform a modification treatment of the conductive carbon black;

[0047] (2) the conductive carbon black pretreatment product obtained in step (1) is mixed uniformly with the remaining processing aids in a weight ratio in a high-speed mixer, and then the substrate in a set weight ratio is added and mixed uniformly at 50° C., wherein the high-speed mixer has a rotation speed controlled between 150 and 250 rpm;

[0048] (3) melt-extrude the mixture obtained in step (2) in a twin-screw extruder at an extrusion temperature of 180° C. and a main engine speed of 120 rpm, and then pelletize and dry to obtain granules;

[0049] (4) The dried granular material obtained in step (3) is placed in a container, and the container is placed in an oven at 65° C. to heat the granular material to 65° C., and then the granular material is mixed with a cross-linking agent of a set weight ratio that is evenly ground, and then placed in an oven at 65° C. for 10 hours to allow the granular material to fully absorb the cross-linking agent, thereby obtaining a high-voltage cable semi-conductive shielding material.

[0050] Example 2

[0051] As a cable semi-conductive shielding material of ionic liquid-modified conductive carbon black according to an embodiment of the present invention, the only difference between this embodiment and embodiment 1 is that the ionic liquid is 2 parts.

[0052] Example 3

[0053] As a cable semi-conductive shielding material of ionic liquid-modified conductive carbon black according to an embodiment of the present invention, the only difference between this embodiment and embodiment 1 is that the ionic liquid is 3 parts.

[0054] Example 4

[0055] As a cable semi-conductive shielding material of ionic liquid-modified conductive carbon black according to an embodiment of the present invention, the only difference between this embodiment and embodiment 1 is that the ionic liquid is 4 parts.

[0056] Comparative Example 1

[0057] As a comparative example of the present invention, a cable semi-conductive shielding material of ionic liquid-modified conductive carbon black is used. The only difference between this comparative example and Example 1 is that the ionic liquid is 0 parts.

[0058] Comparative Example 2

[0059] As a comparative example of the present invention, a cable semi-conductive shielding material of ionic liquid-modified conductive carbon black is used. The only difference between this comparative example and Example 1 is that the dispersant is 1 part of EBS.

[0060] Performance Testing

[0061] The cross-sectional morphology, physical and mechanical properties, electrical properties, and surface smoothness properties of the high-voltage cable semi-conductive shielding materials of Examples 1 to 4 and Comparative Examples 1 to 2 are shown below.

[0062] Table 1 Physical and mechanical properties and electrical properties of the embodiments and comparative examples

[0063]

[0064] As can be seen from Table 1, the semi-conductive shielding material of the high-voltage cable prepared by the present invention exhibits excellent mechanical properties and electrical properties. The mechanical properties, resistivity and surface finish of the semi-conductive shielding material of Example 4 are optimal, the tensile strength of the shielding material reaches 16.3MPa, the elongation at break reaches 321.6%, and the resistivity at 23°C and 90°C is 8.5Ω·cm and 60.3Ω·cm respectively, and its performance is better than that of Comparative Example 2. This is because when the ionic liquid is used for the non-covalent modification of the conductive carbon black, the hydrophobic part is wrapped on the conductive carbon black through the van der Waals force and non-covalent interactions such as π-π, and the hydrophilic part is directly combined with the polar end of the matrix, thereby enhancing the dispersibility. These non-covalent modifications increase the uniform dispersion stability of the conductive carbon black in the matrix resin, reduce the agglomeration phenomenon of the conductive carbon black in the matrix resin, and improve the electrical properties and mechanical properties of the shielding material at the same time; at the same time, the ionic liquid, due to its own good conductivity, helps to improve the conductivity and stability of the semi-conductive shielding material. In addition, ionic liquids act as lubricants and can significantly reduce the dynamic and static friction coefficients of high-voltage cable semi-conductive shielding materials, reduce surface scratches on semi-conductive shielding materials, and improve their processing performance and extrusion surface smoothness.

[0065] Example 4 is compared and analyzed with Comparative Example 2. Compared with the traditional dispersant and dispersion method, it can be seen that the preparation method of the conductive carbon black filler modified by ionic liquid can significantly improve the surface smoothness of the semi-conductive shielding material of the high-voltage cable, and the number of protrusions larger than 50 microns on the surface is reduced from 7 to 0. This is because the preparation method of the highly dispersed conductive carbon black filler is to disperse the conductive carbon black at the molecular level, which can make the conductive carbon black fully contact with the ionic liquid and inhibit the agglomeration of the conductive carbon black particles, thereby increasing the surface smoothness of the semi-conductive shielding material of the high-voltage cable.

[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention and do not limit the protection scope of the present invention. Without departing from the technical solution of the present invention, any modification of the present invention that can be easily implemented by ordinary technicians in this field will fall within the scope of the claims of the present invention.

Claims

1. A cable semi-conductive shielding material of ionic liquid modified conductive carbon black, comprising a substrate, conductive carbon black, a cross-linking agent, an antioxidant, a lubricant, and an ionic liquid; characterized in that: The weight parts of each component are as follows: 58-64 parts of base material, 27-35 parts of conductive carbon black, 1-5 parts of ionic liquid, 1-2 parts of lubricant, 0.3-0.7 parts of antioxidant, 0.4-2.2 parts of cross-linking agent; The ionic liquid is an imidazole ionic liquid; The preparation method of the ionic liquid modified conductive carbon black comprises the following steps: Step 1, remove moisture from the conductive carbon black according to the weight ratio, set the oven temperature to 100°C~120°C, and dry for 4~5 hours; Step 2: Take 300-400 ml of deionized water in a beaker, add the ionic liquid into the deionized water according to the weight ratio, and stir evenly with a magnetic stirrer at a speed of 70-100 rpm for 10-15 min; Step 3, slowly pour the conductive carbon black in step 1 into the dispersion obtained in step 2 according to the weight ratio, stir for 30 minutes, and then let it stand for a period of time, the standing time is 15 minutes; Step 4, after the stirring is completed, ultrasonically disperse the mixed solution of the ionic liquid and the conductive carbon black in an ultrasonic disperser for 1 to 2 hours to obtain a dispersed suspension of the ionic liquid modified conductive carbon black; Step 5, placing the dispersed suspension in step 4 into an oven for drying to obtain highly dispersed ionic liquid modified conductive carbon black, the oven temperature is 110° C. to 130° C., and the drying time is 12 h to 24 h.

2. The cable semi-conductive shielding material of ionic liquid modified conductive carbon black according to claim 1, characterized in that: The substrate is one or more of ethylene-butyl acrylate or ethylene-ethyl acrylate, and the substrate performance is regulated according to the content of the second copolymerized monomer, and the mass ratio of the second copolymerized monomer in the substrate is controlled to be between 16 and 20%.

3. The cable semiconductive shielding material of ionic liquid modified conductive carbon black according to claim 1 or 2, characterized in that: The conductive carbon black is a high-purity conductive carbon black, with a DBP absorption value of 150-170 ml / 100g, an ash content of less than 0.2%, a 325-mesh sieve residue content of less than 8 ppm, and does not contain any excess impurities.

4. The cable semi-conductive shielding material of ionic liquid modified conductive carbon black according to claim 1, characterized in that: The cross-linking agent is dicumyl peroxide.

5. The cable semi-conductive shielding material of ionic liquid modified conductive carbon black according to claim 1, characterized in that: The lubricant is one or more of zinc stearate and pentaerythritol.

6. The cable semi-conductive shielding material of ionic liquid modified conductive carbon black according to claim 1, characterized in that: The antioxidant is one or more of the antioxidant 1010 and the antioxidant 300 .

7. A method for preparing a cable semiconductive shielding material of ionic liquid modified conductive carbon black according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: Step a, mixing the highly dispersible ionic liquid modified conductive carbon black with the lubricant and the antioxidant in a high-speed mixer according to the weight ratio, and then adding the substrate in a set weight ratio and mixing at 45-50° C., wherein the high-speed mixer is controlled at a speed between 150-250 rpm; Step b, melt-extrude the mixture obtained in step a in a twin-screw extruder at an extrusion temperature of 180° C. and a main engine speed of 120 rpm, and then pelletize and dry to obtain a granular material; Step c, putting the dried granules obtained in step b into a container, placing it in a 65°C oven to heat the granules to 65°C, then mixing the granules with a uniformly ground cross-linking agent of a set weight ratio, and then placing it in a 65°C oven for 10 hours to allow the granules to fully absorb the cross-linking agent, thereby obtaining a cable semi-conductive shielding material.