A non-quenched and tempered high-strength steel and its preparation process
By adjusting the proportion of trace elements and the temperature-controlled rolling process, the non-quenched and tempered high-strength steel prepared is mainly composed of pearlite and ferrite, which solves the problem of insufficient strength of existing non-quenched and tempered steel and achieves high yield strength and resistance. Improved tensile strength and hardness, with excellent mechanical properties.
Patent Information
- Application Number
- CN202310049107.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-01
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-02-01
AI Technical Summary
The existing non-quenched and tempered steel has insufficient yield strength and tensile strength, making it difficult to reach the performance level of quenched and tempered steel. Especially large-size steel and steel with poor hardenability have problems such as bending during the quenching and tempering process.
By adjusting the proportion of trace elements, non-quenched and tempered high-strength steel containing carbon, silicon, manganese, phosphorus, chromium, nickel, molybdenum, vanadium, boron and other elements is prepared, and a temperature-controlled rolling process is used, with the final rolling temperature controlled at 800 -850℃, cooling rate is 4-6℃/s, forming steel mainly composed of pearlite and ferrite.
Significantly improve the yield strength and tensile strength of non-quenched and tempered steel. The yield strength can reach 1758MPa, the tensile strength can reach 1800MPa, the HRC hardness can reach 46, and the elongation can reach 46%. It has good mechanical properties and surpasses Performance of most non-quenched and tempered steels on the market.
Smart Images

Figure CN116121648B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nonferrous metal production, in particular to non-quenched and tempered high-strength steel and a preparation process thereof. Background Art
[0002] The heat treatment method of high temperature tempering after quenching is called quenching and tempering. Quenching and tempering can adjust the properties and material of steel to a great extent. Its strength, plasticity and toughness are good, and it has good comprehensive mechanical properties. However, due to factors such as the size of the workpiece, not all steels are suitable for quenching and tempering. For example, some large-sized steels are difficult to put into heat treatment equipment, long rod-shaped steels will bend during the quenching and tempering process, and some steels with poor hardenability are not suitable for quenching and tempering.
[0003] Non-quenched and tempered steel is made by adding vanadium, titanium and niobium microalloying elements to medium carbon manganese steel, which are dissolved in austenite during heating, because the solid solubility of vanadium, titanium and niobium in austenite decreases with cooling. Microalloying elements vanadium, titanium and niobium will precipitate in the first precipitated ferrite and pearlite in the form of fine carbides and nitrides. These precipitates maintain a coherent relationship with the parent phase, strengthening the steel. However, the strength, elongation and other properties of existing non-quenched and tempered steels are still different from those of quenched and tempered steels. The yield strength and tensile strength of most non-quenched and tempered steels do not exceed 1000MPa.
[0004] CN109763601A discloses a non-quenched and tempered steel with a maximum yield strength of 872MPa, a tensile strength of more than 1100MPa, and an elongation of not less than 14%. Compared with other non-quenched and tempered steels, the performance is improved, but there is still a gap with quenched and tempered steels. Summary of the invention
[0005] The purpose of the present invention is to provide a non-quenched and tempered high-strength steel and a preparation process thereof, wherein the prepared non-quenched and tempered steel has higher yield strength and tensile strength than the existing non-quenched and tempered steel, so as to solve the problem of insufficient strength of the non-quenched and tempered steel.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A non-quenched and tempered high-strength steel, comprising the following components by weight: carbon 0.25%-0.35%, silicon 0.05%-0.15%, manganese 2.5%-3.0%, phosphorus 0.03%-0.10%, sulfur ≤0.02%, chromium 0.75%-1.25%, nickel 0.35%-0.65%, molybdenum 0.3%-0.6%, vanadium 0.2%-0.6%, boron 0.0005%-0.0015%, and the balance is iron and unavoidable impurities.
[0008] Preferably, the alloy comprises the following components by weight: 0.30% carbon, 0.1% silicon, 2.6% manganese, 0.05% phosphorus, 0.01% sulfur, 1.0% chromium, 0.5% nickel, 0.5% molybdenum, 0.4% vanadium, 0.0008% boron, and the remainder is iron and inevitable impurities.
[0009] Preferably, the yield strength of the non-quenched and tempered high-strength steel is not less than 1700 MPa.
[0010] Preferably, the tensile strength of the non-quenched and tempered high-strength steel is not less than 1800 MPa.
[0011] Preferably, the HRC hardness of the non-quenched and tempered high-strength steel is not less than 42.
[0012] The present invention also provides a method for preparing non-quenched and tempered high-strength steel, comprising the following steps:
[0013] S1: mixing the raw materials according to the ingredients, smelting the raw materials to obtain steel billets;
[0014] S2: rolling and cooling the steel billet to obtain non-quenched and tempered high-strength steel.
[0015] Preferably, the rolling is temperature-controlled rolling, specifically, the final rolling temperature is controlled at 800-850°C.
[0016] Preferably, the cooling rate is 4-6°C / s.
[0017] In the present invention, copper, nickel and vanadium can improve the strength and yield ratio of steel, silicon and phosphorus can improve the strength of steel, chromium can increase the hardness, and manganese can improve the strength of steel.
[0018] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0019] The present invention adjusts the proportion of various trace elements and adopts appropriate production processes. The non-quenched and tempered high-strength steel prepared by the present invention is mainly composed of pearlite and ferrite. The yield strength can reach 1758MPa and the tensile strength can reach 1800MPa, which are higher than the strength of most non-quenched and tempered steel products on the market. It also has the advantage of high hardness, with an HRC hardness of up to 46 and an elongation of up to 46%, and has good mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a metallographic photograph of the high-strength steel prepared according to the recipe in Example 3 and the process of Example 9.
[0021] Figure 2 This is a metallographic photograph of the high-strength steel prepared according to the recipe in Example 3 and the process of Example 8.
[0022] Figure 3 This is a metallographic photograph of the high-strength steel prepared according to the recipe in Example 4 and the process of Example 7. DETAILED DESCRIPTION
[0023] The present invention provides a non-quenched and tempered high-strength steel, which comprises the following components by weight: 0.25% to 0.35% carbon, 0.05% to 0.15% silicon, 2.5% to 3.0% manganese, 0.03% to 0.10% phosphorus, ≤0.02% sulfur, 0.75% to 1.25% chromium, 0.35% to 0.65% nickel, 0.3% to 0.6% molybdenum, 0.2% to 0.6% vanadium, 0.0005% to 0.0015% boron, and the balance is iron and unavoidable impurities.
[0024] The present invention also provides a method for preparing non-quenched and tempered high-strength steel, comprising the following steps:
[0025] S1: preparing materials according to the composition, smelting the raw materials, the smelting steps including converter smelting → refining → continuous casting, to obtain steel billets;
[0026] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 800-850°C, and then cooled at a cooling rate of 4-6°C / s to obtain non-quenched and tempered high-strength steel.
[0027] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Example 1
[0028] The present embodiment provides a non-quenched and tempered high-strength steel, which comprises the following components by weight: 0.20% carbon, 0.02% silicon, 2.0% manganese, 0.02% phosphorus, 0.012% sulfur, 0.50% chromium, 0.30% nickel, 0.2% molybdenum, 0.1% vanadium, 0.0005% boron, and the balance is iron and unavoidable impurities. Example 2
[0029] The present embodiment provides a non-quenched and tempered high-strength steel, which comprises the following components by weight: 0.25% carbon, 0.05% silicon, 2.5% manganese, 0.03% phosphorus, 0.01% sulfur, 0.75% chromium, 0.35% nickel, 0.3% molybdenum, 0.2% vanadium, 0.0005% boron, and the balance is iron and unavoidable impurities. Example 3
[0030] The present embodiment provides a non-quenched and tempered high-strength steel, which comprises the following components by weight: 0.30% carbon, 0.1% silicon, 2.6% manganese, 0.05% phosphorus, 0.01% sulfur, 1.0% chromium, 0.5% nickel, 0.5% molybdenum, 0.4% vanadium, 0.0008% boron, and the balance is iron and unavoidable impurities. Example 4
[0031] The present embodiment provides a non-quenched and tempered high-strength steel, which comprises the following components by weight: 0.35% carbon, 0.15% silicon, 3.0% manganese, 0.10% phosphorus, 0.013% sulfur, 1.25% chromium, 0.65% nickel, 0.6% molybdenum, 0.6% vanadium, 0.0015% boron, and the remainder is iron and unavoidable impurities. Example 5
[0032] The present embodiment provides a non-quenched and tempered high-strength steel, which comprises the following components by weight: 0.40% carbon, 0.20% silicon, 3.5% manganese, 0.15% phosphorus, 0.013% sulfur, 1.50% chromium, 0.75% nickel, 0.8% molybdenum, 0.8% vanadium, 0.0020% boron, and the remainder is iron and unavoidable impurities. Example 6
[0033] This embodiment provides a method for preparing non-quenched and tempered high-strength steel, comprising the following steps:
[0034] S1: preparing materials according to the composition, smelting the raw materials, the smelting steps including converter smelting → refining → continuous casting, to obtain steel billets;
[0035] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 800°C, and then cooled at a cooling rate of 4°C / s to obtain non-quenched and tempered high-strength steel. Example 7
[0036] This embodiment provides a method for preparing non-quenched and tempered high-strength steel, comprising the following steps:
[0037] S1: preparing materials according to the composition, smelting the raw materials, the smelting steps including converter smelting → refining → continuous casting, to obtain steel billets;
[0038] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 820°C, and then cooled at a cooling rate of 5°C / s to obtain non-quenched and tempered high-strength steel. Example 8
[0039] This embodiment provides a method for preparing non-quenched and tempered high-strength steel, comprising the following steps:
[0040] S1: preparing materials according to the composition, smelting the raw materials, the smelting steps including converter smelting → refining → continuous casting, to obtain steel billets;
[0041] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 850°C, and then cooled at a cooling rate of 6°C / s to obtain non-quenched and tempered high-strength steel. Example 9
[0042] This embodiment provides a method for preparing non-quenched and tempered high-strength steel, comprising the following steps:
[0043] S1: preparing materials according to the composition, smelting the raw materials, the smelting steps including converter smelting → refining → continuous casting, to obtain steel billets;
[0044] S2: The steel billet is subjected to temperature-controlled rolling, the final rolling temperature is controlled at 850°C, and then cooled at a cooling rate of 5°C / s to obtain non-quenched and tempered high-strength steel.
[0045] The proportions of ingredients in Examples 1-5 were used to prepare non-quenched and tempered high-strength steel according to the preparation methods in Examples 6-9, and the yield strength Rm and tensile strength ReL thereof were shown in Tables 1 and 2, respectively:
[0046] Table 1 Yield strength of different non-quenched and tempered high strength steels
[0047] Method Rm / MPa ratio Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 1420 1586 1622 1613 1607 Example 7 1467 1630 1680 1669 1673 Example 8 1478 1691 1758 1732 1733 Example 9 1495 1680 1741 1726 1728
[0048] As shown in Table 1 above, the yield strength of the non-quenched and tempered high-strength steels prepared according to the raw material ratios of Examples 2 to 5 is higher than 1550 MPa, and the maximum yield strength can reach 1758 MPa.
[0049] Table 2 Tensile strength of different non-quenched and tempered high strength steels
[0050] MethodReL / MPa ratio Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 1508 1710 1734 1740 1731 Example 7 1522 1732 1756 1768 1757 Example 8 1548 1765 1795 1781 1789 Example 9 1561 1772 1800 1786 1791
[0051] As shown in Table 2 above, the tensile strength of the non-quenched and tempered high-strength steels prepared according to the raw material ratios of Examples 2 to 5 is higher than 1700 MPa, and the maximum tensile strength can reach 1800 MPa.
[0052] The HRC hardness and elongation of the non-quenched and tempered high-strength steels prepared according to the raw material ratios of Examples 2 to 5 were tested, as shown in Tables 3 and 4 below:
[0053] Table 3 HRC hardness of different non-quenched and tempered high strength steels
[0054] Method HRC ratio Example 2 Example 3 Example 4 Example 5 Example 6 31 34 37 39 Example 7 34 36 40 42 Example 8 37 39 46 44 Example 9 33 37 44 41
[0055] As shown in Table 3 above, the HRC hardness of the non-quenched and tempered high-strength steels prepared in Examples 2 to 5 is higher than 30, and the highest HRC hardness can reach 46.
[0056] Table 4 Elongation of different non-quenched and tempered high-strength steels (elongation δ5)
[0057] Method Elongation / % Ratio Example 2 Example 3 Example 4 Example 5 Example 6 12.6 13.4 13.7 13.5 Example 7 13.1 13.8 14.2 13.8 Example 8 12.8 13.5 13.6 13.4 Example 9 12.5 13.1 13.4 13.6
[0058] As shown in Table 4 above, the δ5 elongation of the non-quenched and tempered high-strength steels prepared in Examples 2 to 5 is higher than 12.5%, and the maximum elongation is 14.2%, which shows good ductility.
[0059] Table 5 Sectional reduction of different non-quenched and tempered high-strength steels
[0060] Method Sectional shrinkage / % Ratio Example 2 Example 3 Example 4 Example 5 Example 6 47.3 48.5 49.6 48.7 Example 7 46.9 47.8 49.3 48.2 Example 8 45.6 47.4 48.7 47.7 Example 9 45.3 47.2 48.2 47.9
[0061] As shown in Table 4 above, the non-quenched and tempered high-strength steels prepared in Examples 2 to 5 have a cross-sectional shrinkage rate higher than 45%, with the maximum cross-sectional shrinkage rate reaching 49.6%, and have good plasticity.
[0062] Figure 1 This is a metallographic photograph of the high-strength steel prepared according to the process of Example 9 using the recipe in Example 3. Figure 2 This is a metallographic photograph of the high-strength steel prepared according to the process of Example 8 using the recipe in Example 3. Figure 3 This is a metallographic photograph of the high-strength steel prepared by the process of Example 7 according to the formulation in Example 4. As shown in the figure, the non-quenched and tempered steel prepared by the formulation and preparation method of the present invention is mainly composed of pearlite and ferrite, among which the proportion of pearlite is much higher than that of general non-quenched and tempered steel, and most of the ferrite is wrapped inside, so that the yield strength and tensile strength of the steel are significantly higher than those of general non-quenched and tempered steel.
[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A non-quenched and tempered high-strength steel, characterized in that: It is composed of the following components by weight: carbon 0.3%~0.35%, silicon 0.1%~0.15%, manganese 2.6%~3.0%, phosphorus 0.03%~0.10%, sulfur ≤0.02%, chromium 0.75%~1.25%, nickel 0.35%~0.65%, molybdenum 0.3%~0.6%, vanadium 0.4%~0.6%, boron 0.0005%~0.0015%, and the balance is iron and unavoidable impurities; The preparation method of the non-quenched and tempered high-strength steel is as follows: S1: mixing the raw materials according to the ingredients, smelting the raw materials to obtain steel billets; S2: rolling and cooling the steel billet to obtain non-quenched and tempered high-strength steel; The final rolling temperature of the non-quenched and tempered high-strength steel is controlled at 800-850°C, and the cooling rate is 4-6°C / s.
2. The non-quenched and tempered high-strength steel according to claim 1, characterized in that: It is composed of the following components by weight: 0.30% carbon, 0.1% silicon, 2.6% manganese, 0.05% phosphorus, 0.01% sulfur, 1.0% chromium, 0.5% nickel, 0.5% molybdenum, 0.4% vanadium, 0.0008% boron, and the balance is iron and inevitable impurities.
3. A non-quenched and tempered high strength steel as claimed in claim 1 or 2, characterized in that: The yield strength of the non-quenched and tempered high-strength steel is not less than 1700 MPa.
4. A non-quenched and tempered high strength steel as claimed in claim 1 or 2, characterized in that: The tensile strength of the non-quenched and tempered high-strength steel is not less than 1800 MPa.
5. The non-quenched and tempered high strength steel according to claim 1 or 2, characterized in that: The HRC hardness of the non-quenched and tempered high-strength steel is not less than 42.
Citation Information
Cited By
Nb-Ti composite microalloyed non-quenched and tempered steel and preparation method thereof
CN119899982A