Filled automotive polypropylene compositions containing recycled content
By replacing complex heterophasic propylene copolymers in the automotive industry with polypropylene-polyethylene blends derived from post-consumer recycled materials and increasing the amount of inorganic fillers, the mechanical properties and odor issues of recycled materials in automotive applications are achieved. Performance enhancement and VOC reduction of the composition.
Patent Information
- Application Number
- CN202180059266.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-13
- Filing Date
- 2021-08-11
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-08-11
AI Technical Summary
Existing recycled polyolefin materials in the automotive industry limit their use in automotive applications due to limited mechanical properties, odor and emission problems, and it is difficult to achieve the preparation of pure polymers and the complete separation of polypropylene and polyethylene.
The complex heterophasic polypropylene copolymer is replaced by a post-consumer recycled polypropylene-polyethylene blend, the amount of inorganic filler is increased, and the impact properties and mechanical properties of the composition are improved by adjusting the component ratio and performance characteristics of the composition. .
It reduces the amount of original heterophasic propylene copolymer, reduces the total amount of the composition, improves the impact characteristics and mechanical properties of the composition, reduces the VOC content, and is suitable for automotive applications.
Smart Images

Figure GDA0004113648690000191 
Figure GDA0004113648690000201 
Figure GDA0004113648690000211
Abstract
Description
Technical Field
[0001] The present invention relates to a polypropylene-based composition containing an inorganic filler and a regenerated material suitable for use in the automotive industry. Background Art
[0002] Compositions suitable for use in the automotive industry usually contain one or more heterophasic polypropylene copolymers, and / or random heterophasic copolymers, a plastomer as an impact modifier and usually some inorganic filler.
[0003] A fundamental problem in the polymer business is regeneration. At present, the market for regenerates, especially regenerates from household waste, usually denoted PCR ("post-consumer resin"), is somewhat limited. Starting from household waste, the sorting and separation methods adopted will not allow the preparation of pure polymers, i.e. there are always some contaminants, or the method may even result in blends of different polymers. When it comes to polyolefins, which constitute the vast majority of the polymer fraction of collected domestic waste, the complete separation of polypropylene and polyethylene is almost impossible. Recycled polyolefin materials, especially post-consumer resins, are often cross-contaminated by non-polyolefin materials such as polyethylene terephthalate, polyamide, polystyrene or non-polymeric substances such as wood, paper, glass or aluminum. Even worse, those post-consumer recycled polyolefin materials are easily available on a multi-ton scale, but unfortunately have limited mechanical properties and often serious odor and / or emission problems.
[0004] In addition to the required mechanical properties, odor and emissions are also very critical for the automotive industry, and there is a trend to further increase the requirements. This greatly limits the use of regenerants in automotive applications.
[0005] However, there is a profound need to allow the dumping and reuse of post-consumer polyolefin regrind in final products without health and safety risks.
[0006] The present invention is based on the surprising finding that complex heterophasic polypropylene copolymers can be at least partially replaced by polypropylene-polyethylene blends derived from post-consumer recycled polyolefin streams, even with benefits regarding impact and VOC properties. Summary of the invention
[0007] The present invention provides a composition suitable for automotive applications, which composition can be obtained by blending components a) to f):
[0008] a) 5.0 to 45 wt%, preferably 9.0 to 42 wt%, more preferably 10 to 40 wt% of a first heterophasic polypropylene copolymer (HECO 1),
[0009] b) 2.0 to 20 wt%, preferably 2.5 to 18 wt%, more preferably 3.0-17 wt% of a second heterophasic polypropylene copolymer (HECO2),
[0010] c) 10 to 60 wt%, preferably 12-55 wt%, more preferably 14 to 52 wt% of a polypropylene-polyethylene blend (A),
[0011] d) 2.5 to 25 wt%, preferably 5.0 to 22 wt% and more preferably 6.5-20 wt% of an ethylene-based elastomer,
[0012] e) 5.0 to 30 wt%, preferably 7.0-25 wt%, more preferably 8.5 to 20 wt% of an inorganic filler,
[0013] f) 0.1 to 4.0 wt% of additives,
[0014] wherein all percentages refer to the total composition, and wherein,
[0015] (i) the first heterophasic polypropylene copolymer (HECO 1) comprises a matrix phase and an elastomeric phase dispersed therein, the first heterophasic polypropylene copolymer (HECO 1) having:
[0016] - a melt flow rate MFR2 (230°C, ISO 1133) of 75 to 200 g / 10 min, preferably 80 to 150 g / 10 min, more preferably 85 to 120 g / 10 min; and
[0017] - the intrinsic viscosity of the xylene cold soluble (XCS) fraction (measured in decalin at 135° C. according to DIN ISO 1628 / 1) is from 1.2 to 3.2 dl / g, preferably from 1.4 to 3.1 dl / g, more preferably from 1.5 to 3.0 dl / g; and
[0018] (ii) the second heterophasic polypropylene copolymer (HECO2) comprises a matrix phase and an elastomeric phase dispersed therein, the second heterophasic polypropylene copolymer (HECO2) having:
[0019] - a melt flow rate MFR2 (230°C, ISO 1133) of 2.5 to 10 g / 10 min, preferably 3.0 to 8.5 g / 10 min, more preferably 3.5 to 7.5 g / 10 min; and
[0020] - the intrinsic viscosity of the xylene cold soluble fraction (XCS) (measured in decalin at 135° C. according to DIN ISO 1628 / 1) is from 4.0 to 10 dl / g, preferably from 5.0 to 9.0 dl / g, more preferably from 5.5 to 8.5 dl / g; and
[0021] (iii) The polypropylene-polyethylene blend (A) comprises:
[0022] A-1) Polypropylene,
[0023] A-2) Polyethylene,
[0024] wherein the weight ratio of polypropylene to polyethylene is from 19:1 to 7:3, and the polypropylene-polyethylene blend (A) has:
[0025] - a melt flow rate MFR2 (230°C, ISO 1133) of 5.0 to 30 g / 10 min, preferably 7.0 to 26 g / 10 min, more preferably 9.0 to 23 g / 10 min; and
[0026] - xylene cold soluble fraction (XCS) from 2.0 to 15 wt%, preferably from 2.5 to 13 wt%, more preferably from 3.0 to 11 wt% (ISO 16152, 1st edition, 25° C.); and
[0027] - Optionally, the residual ash content is less than 3.0 wt%, preferably 0.5 to 2.7 wt%, more preferably 0.7 to 2.5 wt%,
[0028] The polypropylene-polyethylene blend (A) optionally has one or more of the following properties:
[0029] (aa) a limonene content of 0.1 ppm to 100 ppm, preferably 0.1 ppm to 50 ppm, more preferably 0.1 ppm to 20 ppm, most preferably 0.1 ppm to 5 ppm as determined by solid phase microextraction (HS-SPME-GC-MS);
[0030] (bb) a fatty acid content of 0.1 to 100 ppm as determined by solid phase microextraction (HS-SPME-GC-MS);
[0031] (cc) a polyamide content of 0.05 to 1.5 wt % as determined by NMR;
[0032] (dd) a polystyrene content of 0.05-3.0 wt % as determined by NMR;
[0033] in,
[0034] -The ethylene-based elastomer is selected from C2C4 elastomer, C2C6 elastomer and / or C2C8 elastomer, preferably, the ethylene-based elastomer is C2C4 elastomer, the ethylene-based elastomer:
[0035] - having a melt flow rate MFR2 (190°C, ISO1133) of 0.05 to 5.0 g / 10 min, preferably 0.1 to 4.5 g / 10 min
[0036] -With 850 to 885 kg / m 3 , preferably 855 to 875 kg / m 3 density; and
[0037] (iv) an inorganic filler, preferably talc,
[0038] - has a median particle size d50 of 0.3 to 3.0 microns, more preferably 0.5 to 2.5 microns before compounding;
[0039] - Preferably, before compounding, the top cut particle size d 95 1.0 to 8.0 microns,
[0040] The amount of components a) to e) is at least 90 wt%, preferably at least 95 wt%, most preferably at least 96 wt% of the composition suitable for automotive applications.
[0041] More specifically, the present invention provides a composition suitable for automotive applications obtainable by blending at least components a) to f):
[0042] a) 5.0 to 45 wt%, preferably 9.0 to 42 wt%, more preferably 10 to 40 wt% of a first heterophasic polypropylene copolymer (HECO 1),
[0043] b) 2.0 to 20 wt%, preferably 2.5 to 18 wt%, more preferably 3.0 to 17 wt% of a second heterophasic polypropylene copolymer (HECO2),
[0044] c) 10 to 60 wt%, preferably 12-55 wt%, more preferably 14 to 52 wt% of a polypropylene-polyethylene blend (A),
[0045] d) 2.5 to 25 wt%, preferably 5.0 to 22 wt%, more preferably 6.5-20 wt% of an ethylene-based elastomer,
[0046] e) 5.0 to 30 wt%, preferably 7.0-25 wt%, more preferably 8.5 to 20 wt% of an inorganic filler,
[0047] f) 0.1 to 4.0 wt% of additives,
[0048] wherein all percentages refer to the total composition, wherein,
[0049] (i) the first heterophasic polypropylene copolymer (HECO 1) comprises a matrix phase and an elastomeric phase dispersed therein, the first heterophasic polypropylene copolymer (HECO 1) having:
[0050] - a melt flow rate MFR2 (230°C, ISO 1133) of 75 to 200 g / 10 min, preferably 80 to 150 g / 10 min, more preferably 85 to 120 g / 10 min;
[0051] - 8.0 to 20.0 wt %, preferably 10 to 19 wt %, more preferably 12 to 18 wt % of xylene cold soluble fraction (XCS) (ISO 16152, 1st edition, 25° C.);
[0052] - the intrinsic viscosity of the xylene cold soluble fraction (XCS) (measured in decalin at 135° C. according to DIN ISO 1628 / 1) is from 1.2 to 3.2 dl / g, preferably from 1.4 to 3.1 dl / g, more preferably from 1.5 to 3.0 dl / g; and
[0053] - a melt flow rate MFR2 (230° C., ISO 1133) of the xylene insoluble fraction (XCI) (ISO 16152, first edition, 25° C.) of 100 to 500 g / 10 min, preferably 110 to 400 g / 10 min, more preferably 120 to 300 g / 10 min,
[0054] - a content of units derived from ethylene in the xylene cold soluble fraction (XCS) of 25.0 to 50.0 wt%, preferably 28.0 to 45.0 wt%, more preferably 30.0 to 42.0 wt%,
[0055] - a total content of units derived from ethylene of 2.0 to 13.0 wt%, preferably 2.8 to 10.0 wt%, more preferably 3.5 to 9.0 wt%, and
[0056] (ii) the second heterophasic polypropylene copolymer (HECO2) comprises a matrix phase and an elastomeric phase dispersed therein, the second heterophasic polypropylene copolymer (HECO2) having:
[0057] - a melt flow rate MFR2 (230°C, ISO 1133) of 2.5 to 10 g / 10 min, preferably 3.0 to 8.5 g / 10 min, more preferably 3.5 to 7.5 g / 10 min;
[0058] - 20 to 50 wt%, preferably 21 to 45 wt%, more preferably 22 to 40 wt% of xylene cold soluble fraction (XCS) (ISO 16152, first edition, 25 ° C);
[0059] - the intrinsic viscosity of the xylene cold soluble fraction (XCS) (measured in decalin at 135° C. according to DIN ISO 1628 / 1) is from 4.0 to 10 dl / g, preferably from 5.0 to 9.0 dl / g, more preferably from 5.5 to 8.5 dl / g; and
[0060] - a xylene insoluble fraction (XCI) (ISO 16152, first edition, 25° C.) having a melt flow rate MFR2 of 20 to 90 g / 10 min, preferably 25 to 80 g / 10 min, more preferably 30 to 70 g / 10 min, and
[0061] - a content of units derived from ethylene in the xylene cold soluble fraction (XCS) of 15.0 to 25.0 wt%, preferably 17.0 to 24.0 wt%, more preferably 19.0 to 23.5 wt%,
[0062] The total content of units derived from ethylene is from 3.0 to 15.0 wt%, preferably from 3.5 to 13.0 wt%, more preferably from 4.0 to 11.0 wt%, and
[0063] (iii) The polypropylene-polyethylene blend (A) comprises:
[0064] A-1) Polypropylene,
[0065] A-2) Polyethylene,
[0066] wherein the weight ratio of polypropylene to polyethylene is from 19:1 to 7:3, and the polypropylene-polyethylene blend (A) has:
[0067] - a melt flow rate MFR2 (230°C, ISO 1133) of 5.0 to 30 g / 10 min, preferably 7.0 to 26 g / 10 min, more preferably 9.0 to 23 g / 10 min;
[0068] - xylene cold soluble fraction (XCS) is from 2.0 to 15 wt%, preferably from 2.5 to 13 wt%, more preferably from 3.0 to 11 wt% (ISO 16152, first edition, 25° C.); and
[0069] - Optionally, the residual ash content is less than 3.0 wt%, preferably 0.5 to 2.7 wt%, more preferably 0.7 to 2.5 wt%,
[0070] The polypropylene-polyethylene blend (A) has one or more of the following characteristics:
[0071] (aa) a limonene content of 0.1 ppm to 100 ppm, preferably 0.1 ppm to 50 ppm, more preferably 0.1 ppm to 20 ppm, most preferably 0.1 ppm to 5 ppm as determined by solid phase microextraction (HS-SPME-GC-MS);
[0072] (bb) a fatty acid content of 0.1 to 100 pp as determined by solid phase microextraction (HS-SPME-GC-MS);
[0073] (cc) a polyamide content of 0.05 to 1.5 wt % as determined by NMR;
[0074] (dd) a polystyrene content of 0.05-3.0 wt % as determined by NMR;
[0075] in,
[0076] -The ethylene-based elastomer is selected from C2C4 elastomer, C2C6 elastomer and / or C2C8 elastomer, preferably, the ethylene-based elastomer is C2C4 elastomer, the ethylene-based elastomer:
[0077] - having a melt flow rate MFR2 (190° C., ISO 1133) of 0.05 to 5.0 g / 10 min, preferably 0.1 to 4.5 g / 10 min,
[0078] -With 850 to 885 kg / m 3 , preferably 855 to 875 kg / m 3 density;
[0079] (iv) Inorganic filler, preferably talc
[0080] - having a median particle size d of 0.3 to 3.0 microns, more preferably 0.5 to 2.5 microns before compounding 50 ;
[0081] Preferably, before compounding, the top cut particle size d 95 1.0 to 8.0 microns,
[0082] The amount of components a) to e) is at least 90 wt%, preferably at least 95 wt%, most preferably at least 96 wt% of the composition suitable for automotive applications.
[0083] The present invention also provides an article comprising, preferably consisting of, a composition according to the present invention.
[0084] advantage
[0085] The present invention not only allows to replace complex heterophasic propylene copolymers by recycled polypropylene-polyethylene blends derived from household waste that can be obtained on a large scale, but also allows the amount of fillers (usually talc) to be increased. In other words, it is surprisingly found that the impact properties significantly increased due to the addition of recycled polypropylene-polyethylene blends allow to move towards higher content of fillers for a certain stiffness. Therefore, there are multi-dimensional advantages: mixing recycled polypropylene-polyethylene blends not only allows to reduce the amount of original heterophasic propylene copolymers, but also allows to reduce the total amount of polymers in the composition.
[0086] definition
[0087] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the invention belongs. Although any methods and materials similar or equivalent to those described herein can be used in practice to test the present invention, preferred materials and methods are described herein. In describing and advocating the present invention, the following terms will be used according to the definitions set forth below. Unless otherwise clearly indicated, the use of the term "a" or the like refers to one or more.
[0088] For the purpose of this specification, the term "recycled waste" or "recycled material" is used to refer to materials recovered from both post-consumer waste and industrial waste, in contrast to virgin polymers. Post-consumer waste refers to objects that have completed at least the first use cycle (or life cycle), i.e., have reached their first purpose. In contrast, industrial waste refers to manufacturing waste, respectively conversion waste, which generally does not reach consumers. The term "original" refers to newly produced materials and / or objects before their first use, which have not yet been regenerated. Based on the presence or absence of contaminants such as limonene and / or fatty acids and / or paper and / or wood, virgin materials and post-consumer materials can be easily distinguished. Polypropylene-polyethylene blends can also be distinguished according to their sources by the presence of polystyrene and / or polyamide. Residual content means a content above the detection limit. Many different kinds of polyethylene or polypropylene can be present in "recycled materials". The ratio of polypropylene (A-1) to polyethylene plus polyethylene copolymer (A-2) is experimentally determined by using isotactic polypropylene (iPP) and high-density polyethylene (HDPE) for calibration. Polymer blends are mixtures of two or more polymer components. Typically, blends can be prepared by mixing two or more polymer components. Suitable mixing methods known in the art are post-polymerization blending. Post-polymerization blending can be dry blending of polymer components such as polymer powders and / or compounded polymer pellets or melt blending of polymer components by melt mixing. Propylene random copolymers are copolymers of propylene monomer units and comonomer units, wherein the comonomer units are randomly distributed on the polypropylene chain. "Compatibilizers" are substances in polymer chemistry that are added to a blend of polymers with limited miscibility to improve their stability. "Polypropylene-polyethylene blends" refer to compositions containing both polypropylene and polyethylene, and also include polypropylene copolymers and polyethylene copolymers. Since direct determination of polypropylene content and polyethylene content is impossible, the weight ratio of polypropylene (A-1) to polyethylene (A-2) of 19:1 to 7:3 represents an equivalent ratio determined by calibration of iPP and HDPE and by determination of IR spectra. The term "elastomer" refers to a natural or synthetic polymer with elasticity. The term "XCS" refers to the xylene cold soluble content (XCSwt%) measured at 25°C according to ISO 16152. The term "XCI" refers to the xylene cold insoluble content (XCIwt%) measured at 25°C according to ISO 16152. If not otherwise noted, "%" refers to weight %. The presence of heterogeneous properties can be easily determined by the number of glass transition points. Reactor blends are blends derived from two or more reactors connected in series or produced in a reactor with two or more reaction compartments. Alternatively, reactor blends can be obtained by blending in solution. Reactor blends are contrasted with the compound manufactured by melt extrusion. Ethylene elastomers refer to elastomers consisting of units derived from ethylene whose amount is at least wt%.
[0089] Composition of the present invention
[0090] The compositions suitable for automotive applications according to the invention are particularly suitable for injection molding of articles used in the interior and exterior of vehicles.
[0091] The composition suitable for automotive applications according to the present invention preferably has a melt flow rate (ISO 1133, 2.16 kg, 230° C.) of 10.0 to 25 g / 10 min, more preferably a melt flow rate (ISO 1133, 2.16 kg, 230° C.) of 12.0 to 25 g / 10 min. The melt flow rate of the composition can be easily adjusted by varying the individual amounts of the components, and in particular can be adjusted by selecting a polypropylene-polyethylene blend (A) having an appropriate melt flow rate.
[0092] On the other hand, the composition suitable for automotive applications according to the invention preferably has a tensile modulus of 1300 to 1700 MPa (ISO 527.2; 23° C.) The final tensile modulus can be fine-tuned by the amount of filler, whereby a higher amount of filler will result in a higher tensile modulus.
[0093] The composition suitable for automotive applications according to the present invention has one or more of the following characteristics:
[0094] (aa) residual amount of limonene;
[0095] (bb) residual amounts of fatty acids;
[0096] (cc) residual amounts of polyamide;
[0097] (dd) Residual amount of polystyrene.
[0098] These residual amounts are introduced via the admixture of the polypropylene-polyethylene blend (A) with polypropylene-polyethylene blends (A) originating from consumer waste. The presence of such residual material can be used as a way to distinguish the admixture of polypropylene-polyethylene blends (A) originating from consumer waste from the admixture of polypropylene-polyethylene blends (A) originating from industrial waste. In other words, the above allows a distinction to be made between post-consumer recycled (PCR) and post-industrial recycled (PIR).
[0099] Compositions suitable for automotive applications according to the invention preferably have a VOC of less than 75 μg / gram of composition, measured on material obtained directly from extrusion after a process as described in VDA 278. Without wishing to be bound by theory, the applicant believes that in a first aspect, the presence of fillers, in particular talc, is beneficial. In a second aspect, the incorporation of the polypropylene-polyethylene blend (A) also reduces the overall VOC content, since the polymers may have lost some amount of VOC in their first use due to being subjected to the elements, i.e. higher temperatures and wind.
[0100] HECO1
[0101] HECO 1 is a heterophasic polypropylene copolymer, i.e. comprises a matrix phase and an elastomeric phase dispersed therein. The first heterophasic polypropylene copolymer (HECO1) has a melt flow rate MFR2 (230°C, ISO 1133) of 75 to 200 g / 10 min, preferably 80 to 150 g / 10 min, more preferably 85 to 120 g / 10 min; and an intrinsic viscosity of the xylene cold soluble fraction (XCS) (measured in decalin at 135°C according to DIN ISO 1628 / 1) of 1.2 to 3.2 dl / g, preferably 1.4 to 3.1 dl / g, more preferably 1.5 to 3.0 dl / g. HECO 1 contributes particularly to the good injection molding properties of the composition. Preferably, HECO1 has:
[0102] - a melt flow rate MFR2 (230°C, ISO 1133) of 75 to 200 g / 10 min, preferably 80 to 150 g / 10 min, more preferably 85 to 120 g / 10 min; and
[0103] - 8.0 to 20.0 wt%, preferably 10 to 19 wt%, more preferably 12 to 18 wt% of xylene cold soluble fraction (XCS) (ISO 16152, first edition, 25° C.); and
[0104] - the intrinsic viscosity of the xylene cold soluble fraction (XCS) (measured in decalin at 135° C. according to DIN ISO 1628 / 1) is from 1.2 to 3.2 dl / g, preferably from 1.4 to 3.1 dl / g, more preferably from 1.5 to 3.0 dl / g; and
[0105] - a melt flow rate MFR2 (230° C., ISO 1133) of the xylene insoluble (XCI) fraction (ISO 16152, first edition, 25° C.) of 100 to 500 g / 10 min, preferably 110 to 400 g / 10 min, more preferably 120 to 300 g / 10 min,
[0106] - the content of units derived from ethylene in the xylene cold soluble fraction (XCS) is from 25.0 to 50.0 wt%, preferably from 28.0 to 45.0 wt%, more preferably from 30.0 to 42.0 wt%,
[0107] The total content of units derived from ethylene is from 2.0 to 13.0 wt%, preferably from 2.8 to 10.0 wt%, more preferably from 3.5 to 9.0 wt%.
[0108] In a particularly preferred embodiment, HECO1 has:
[0109] - Melt flow rate MFR2 (230°C, ISO1133) of 85 to 120 g / 10 min;
[0110] - 12 to 18 wt.% of xylene cold soluble fraction (XCS) (ISO 16152, 1st edition, 25°C);
[0111] - the intrinsic viscosity of the xylene cold soluble fraction (XCS) (measured in decalin at 135° C. according to DIN ISO 1628 / 1) is from 1.5 to 3.0 dl / g;
[0112] - a xylene insoluble (XCI) fraction (ISO 16152, 1st edition, 25° C.) having a melt flow rate MFR2 (230° C., ISO 1133) of 120 to 300 g / 10 min,
[0113] - a content of units derived from ethylene in the xylene cold soluble fraction (XCS) of 30.0 to 42.0 wt %,
[0114] The total content of units derived from ethylene is between 3.5 and 9.0 wt%.
[0115] HECO2
[0116] HECO2 is a heterophasic polypropylene copolymer, i.e. comprising a matrix phase and an elastomeric phase dispersed therein, having a melt flow rate MFR2 (230°C, ISO 1133) of 2.5 to 10 g / 10 min, preferably 3.0 to 8.5 g / 10 min, more preferably 3.5 to 7.5 g / 10 min; and
[0117] The intrinsic viscosity of the xylene cold soluble fraction (XCS) (measured in decalin at 135° C. according to DIN ISO 1628 / 1) is from 4.0 to 10 dl / g, preferably from 5.0 to 9.0 dl / g, more preferably from 5.5 to 8.5 dl / g. HECO 2 differs greatly from HECO 2. HECO 2 contributes particularly to the good surface properties, in particular to the low MSE of the compositions according to the invention.
[0118] Preferably, HECO2 has
[0119] - a melt flow rate MFR2 (230°C, ISO 1133) of 2.5 to 10 g / 10 min, preferably 3.0 to 8.5 g / 10 min, more preferably 3.5 to 7.5 g / 10 min; and
[0120] 20 to 50 wt %, preferably 21 to 45 wt %, more preferably 22 to 40 wt % of xylene cold soluble fraction (XCS) (ISO 16152, first edition, 25° C.);
[0121] - the intrinsic viscosity of the xylene cold soluble fraction (XCS) (measured in decalin at 135° C. according to DIN ISO 1628 / 1) is from 4.0 to 10 dl / g, preferably from 5.0 to 9.0 dl / g, more preferably from 5.5 to 8.5 dl / g;
[0122] - the melt flow rate MFR2 (230° C., ISO 1133) of the xylene insoluble (XCI) fraction (ISO 16152, first edition, 25° C.) is from 20 to 90 g / 10 min, preferably from 25 to 80 g / 10 min, more preferably from 30 to 70 g / 10 min,
[0123] - a content of units derived from ethylene in the xylene cold soluble fraction (XCS) of 15.0 to 25.0 wt%, preferably 17.0 to 24.0 wt%, more preferably 19.0 to 23.5 wt%,
[0124] The total content of units derived from ethylene is from 3.0 to 15.0 wt%, preferably from 3.5 to 13.0 wt%, more preferably from 4.0 to 11.0 wt%.
[0125] In a particularly preferred embodiment, the HECO has:
[0126] - a melt flow rate MFR2 (230°C, ISO 1133) of 3.5 to 7.5 g / 10 min; and
[0127] - 22 to 40% by weight of xylene cold soluble fraction (XCS) (ISO 16152, 1st edition, 25° C.);
[0128] - an intrinsic viscosity of the xylene cold soluble fraction (XCS) of 5.5 to 8.5 dl / g (measured in decalin at 135° C. according to DIN ISO 1628 / 1); and
[0129] - the melt flow rate MFR2 (230° C., ISO 1133) of the xylene insoluble (XCI) fraction (ISO 16152, first edition, 25° C.) is 30 to 70 g / 10 min,
[0130] - a content of units derived from ethylene in the xylene cold soluble fraction (XCS) of from 19.0 to 23.5% by weight, and
[0131] The total content of units derived from ethylene is between 4.0 and 11.0 wt%.
[0132] Ethylene elastomer
[0133] The ethylene-based elastomer is selected from C2C4 elastomers, C2C6 elastomers and / or C2C8 elastomers, and preferably the ethylene-based elastomer is a C2C4 elastomer. Such elastomers are also commonly referred to as plastomers and are commercially available from Dow Chemical, ExxonMobil and Borealis. Independently, the ethylene-based elastomer also has a melt flow rate MFR2 (190°C, ISO1133) of 0.05 to 5.0 g / 10 min, preferably 0.1 to 4.5 g / 10 min, and 850 to 885 kg / m 3 , preferably 855 to 875 kg / m 3 density.
[0134] In a particularly preferred embodiment, the ethylene-based elastomer has a melt flow rate MFR2 (190° C., ISO 1133) of 0.1 to 4.5 g / 10 min and a 3 density.
[0135] The ethylene-based elastomer contributes particularly to the impact properties of the composition of the present invention and may also act as a compatibilizer for the polypropylene-polyethylene blend (A).
[0136] Polypropylene-polyethylene blends (A)
[0137] The polypropylene-polyethylene blend (A) according to the present invention comprises:
[0138] A-1) Polypropylene,
[0139] A-2) Polyethylene,
[0140] The weight ratio of polypropylene to polyethylene is 19:1 to 7:3.
[0141] At the same time, the polypropylene-polyethylene blend (A) has:
[0142] - a melt flow rate MFR2 (230°C, ISO 1133) of 5.0 to 30 g / 10 min, preferably 7.0 to 26 g / 10 min, more preferably 9.0 to 23 g / 10 min; and
[0143] - xylene cold soluble fraction (XCS) is from 2.0 to 15 wt%, preferably from 2.5 to 13 wt%, more preferably from 3.0 to 11 wt% (ISO 16152, first edition, 25° C.); and
[0144] Optionally, the residual ash content is below 3.0 wt%, preferably 0.5 to 2.7 wt%, more preferably 0.7 to 2.5 wt%.
[0145] The polypropylene-polyethylene blend (A) according to the present invention is a recycled material, preferably originating from household waste. It is particularly preferred that the polypropylene-polyethylene blend (A) according to the present invention is derived in an amount of at least 90 wt% from post-consumer waste.
[0146] The polypropylene-polyethylene blend (A) according to the present invention may have one or more of the following properties:
[0147] aa) a limonene content of 0.1 ppm to 100 ppm, preferably 0.1 ppm to 50 ppm, more preferably 0.1 ppm to 20 ppm, most preferably 0.1 ppm to 5 ppm, as determined by solid phase microextraction (HS-SPME-GC-MS);
[0148] bb) a fatty acid content of 0.1 to 100 ppm as determined by using solid phase microextraction (HS-SPME-GC-MS);
[0149] cc) a polyamide content of 0.05 to 1.5 wt % as determined by NMR;
[0150] dd) a polystyrene content of 0.05 to 3.0 wt % as determined by NMR;
[0151] ee) the above mentioned residual ash content.
[0152] It should be understood that the composition of the polypropylene-polyethylene blend (A) can vary widely, i.e. can include polypropylene homopolymer, polypropylene copolymer, polyethylene and polyethylene copolymer. Since direct determination of the polypropylene content and the polyethylene content is not possible, the weight ratio of polypropylene (A-1) to polyethylene (A-2) of 19:1 to 7:3 is an equivalent ratio determined by calibration of iPP homopolymer and HDPE.
[0153] Conventionally, the polypropylene-polyethylene blend (A) according to the present invention may also have one or more of the following:
[0154] - residual content of PET determined as described in the experimental part;
[0155] - residual contents of talc and chalk as described in the experimental part;
[0156] - Residual content of metals (determined by x-ray fluorescence (XRF));
[0157] - a residual amount of paper as described in the experimental part;
[0158] - Residual amounts of wood as described in the experimental part;
[0159] - Total free fatty acid content between 0.1 and 100 ppm measured by using headspace solid phase microextraction (HS-SPME-GC-MS).
[0160] The polypropylene-polyethylene blend (A) according to the present invention is preferably obtained from washing and / or aeration steps known in the art.
[0161] additive
[0162] Additives are generally used in the composition of the present invention. Preferably, the additive is selected from one or more of an antioxidant, a UV stabilizer, a slip agent, a nucleating agent, a pigment, a lubricant, a masterbatch polymer and / or an anti-fogging agent.
[0163] Inorganic fillers
[0164] The inorganic filler, preferably talc, has a median particle size d of 0.3 to 3.0 microns, more preferably 0.5 to 2.5 microns before compounding. 50 ; and preferably having a top cut particle size d of 1.0 to 8.0 microns before compounding 95 Such inorganic fillers are commercially available.
[0165] Paint Adhesion
[0166] Compositions suitable for automotive applications preferably exhibit coating adhesion as measured by coating area of failure or delamination.
[0167] Preferably, compositions suitable for automotive applications have a thickness of less than 24 mm. 2 , preferably 0 to 24 mm 2 , more preferably 0 to 13 mm 2 In mm 2 It is the unit coating area of failure or delamination. DETAILED DESCRIPTION
[0168] Several preferred embodiments will be described below. In a first preferred embodiment, the composition suitable for automotive applications according to the present invention can be obtained by blending at least components a) to f):
[0169] a) 20 to 35 wt% of a first heterophasic polypropylene copolymer (HECO 1),
[0170] b) 5.0 to 20 wt% of a second heterophasic polypropylene copolymer (HECO2),
[0171] c) 20 to 30 wt% of a polypropylene-polyethylene blend (A),
[0172] d) 7.0 to 22 wt%, preferably 11.0 to 20 wt%, of an ethylene elastomer,
[0173] e) 5.0 to 25 wt%, preferably 7.0-20 wt%, more preferably 10-19 wt% of an inorganic filler,
[0174] f) 0.1 to 4.0 wt% of additives.
[0175] Again, the amount of components a) to e) is at least 90 wt%, preferably at least 95 wt%, most preferably at least 96 wt% of the composition suitable for automotive applications.
[0176] All preferred ranges and definitions described above, in particular all ranges and definitions described above for blend (A), also apply to this embodiment.
[0177] The composition of this embodiment preferably has a tensile modulus (ISO 527.2; 23° C.) of 1400 MPa to 1700 MPa, and a tensile strength of at least 40 kJ / m 2 Charpy notched impact strength (non-instrumented, ISO 179-1 at +23°C) of (1eA).
[0178] Independently therefrom but preferably in addition to the above, the composition according to this embodiment has a heat deflection temperature (ISO 75B) of at least 90°C.
[0179] This preferred embodiment is characterized by good stiffness and very good impact resistance with a moderate amount of regenerate.
[0180] In a second preferred embodiment, the composition according to the invention suitable for automotive applications is obtainable by blending at least components a) to f):
[0181] a) 5.0 to 20 wt% of a first heterophasic polypropylene copolymer (HECO 1);
[0182] b) 2.5 to 7.0 wt% of a second heterophasic polypropylene copolymer (HECO2);
[0183] c) 30 to 55 wt% of a polypropylene-polyethylene blend (A);
[0184] d) 7.0 to 22 wt%, preferably 11.0 to 20 wt% of an ethylene elastomer;
[0185] e) 5.0 to 25 wt%, preferably 7.0 to 20 wt%, more preferably 10 to 19 wt% of an inorganic filler; and
[0186] f) 0.1 to 4.0 wt% of additives.
[0187] Again, the amount of components a) to e) is at least 90 wt%, preferably at least 95 wt%, most preferably at least 96 wt% of the composition suitable for automotive applications.
[0188] The composition according to this embodiment preferably has a tensile modulus (ISO 527.2; 23° C.) of 1200-1400 MPa and a thermal conductivity of at least 40 kJ / m 2 Charpy notched impact strength (non-instrumented, ISO 179-1, at +23°C) of (1eA).
[0189] All preferred ranges and definitions described above, in particular all ranges and definitions described above for blend (A), also apply to this embodiment.
[0190] Independently therefrom but preferably in combination therewith, the composition of this embodiment has a melt flow rate (ISO 1133, 2.16 kg, 230° C.) of 6.0 to 15 g / 10 min.
[0191] This preferred second embodiment is characterized by having a moderate stiffness with a very large amount of regenerants and still having a particular impact resistance. This embodiment is particularly suitable for increasing the amount of filler.
[0192] Experimental Section
[0193] The following examples are included to demonstrate certain aspects and embodiments of the present invention as described in the claims. However, it should be understood by those skilled in the art that the following description is illustrative only and should not be considered in any way as limiting the present invention.
[0194] Test Method
[0195] a) Amount of iPP, polystyrene, polyethylene (and copolymers containing ethylene), poly(ethylene terephthalate) and polyamide-6
[0196] To establish different calibration curve standards, iPP and HDPE as well as iPP, PS and PA6 were blended. To quantify the content of foreign polymers, IR spectra were recorded in the solid state using a Bruker Vertex 70 FTIR spectrometer. Films were prepared using a compression molding apparatus at 190 °C with a clamping force of 4-6 MPa. The thickness of the film for the calibration standards for iPP and HDPE was 300 μm, and a film thickness of 50-100 μm was used for the quantification of iPP, PS and PA6. A spectral range of 4000-400 cm -1 , aperture is 6mm, spectral resolution is 2cm -1 , 16 background scans, 16 spectral scans, interferogram zero filling factor of 32 and standard transmission FTIR spectrum of Norton Beer with strong apodization.
[0197] Measured 1167cm in iPP -1 The absorbance of the band at was measured and the iPP content was quantified according to a calibration curve (absorption / thickness (cm) vs. iPP content (wt %)).
[0198] Measured at 1601cm -1 (PS) and 3300cm -1 The absorbance of the band at (iPP + PS + PA6) was measured, and the PS and PA6 contents were quantified according to the calibration curve (absorption / thickness (cm)) vs. PS and PA contents (wt%). The content of the copolymer containing polyethylene and ethylene was obtained by subtracting (iPP + PS + PA6) from 100, taking into account the content of non-polymeric impurities determined in the following method. The analysis was performed as a double determination.
[0199] b) Tensile modulus of rupture and tensile strain
[0200] Determined according to ISO 527-2 (crosshead speed = 1 mm / min; test speed 50 mm / min at 23° C.) using injection molded samples 1B prepared as described in EN ISO 1873-2 (dog bone shape, 4 mm thickness). The measurements were performed after a conditioning time of 96 hours at 23° C.
[0201] c) Impact strength
[0202] 80×10×4mm prepared according to EN ISO1873-2 3 The Charpy notched impact strength was determined according to ISO 179-1eA at +23° C., 0° C. and −20° C. on injection-molded specimens of 1000 nm. The measurement was carried out after a conditioning time of 96 hours at 23° C. on the specimens.
[0203] d) Instrumented puncture test
[0204] According to ISO6603-2:2000, at 23℃, 0℃ and -20℃, for 60×60×1mm 3 The injection molded plaques were subjected to instrumented puncture testing. The measurements were performed after a conditioning time of 96 hours on the samples at 23°C.
[0205] e) Comonomer content
[0206] Poly(propylene-co-ethylene)-ethylene content-IR spectrum
[0207] The ethylene content of poly(ethylene-co-propylene) copolymers was quantified using quantitative infrared (IR) spectroscopy by calibration to the primary method. 13 The calibration was facilitated by a set of in-house non-commercial calibration standards of known ethylene content determined by C solution state nuclear magnetic resonance (NMR) spectroscopy. The calibration procedure was performed in a conventional manner well documented in the literature. The calibration set consisted of 38 calibration standards with ethylene contents ranging from 0.2 to 75.0 wt %, which were produced at pilot scale or full scale under various conditions. The calibration set was selected to reflect the typical variations of copolymers encountered by the final quantitative IR spectroscopy.
[0208] Quantitative IR spectra were recorded in the solid state using a Bruker Vertex 70 FTIR spectrometer. Spectra were recorded on 300 μm thick 25×25 mm square films prepared by compression molding at 180-210° C. and 4-6 MPa. For samples with very high ethylene content (>50 mol%), 100 μm thick films were used. A 5000-500 cm -1 spectral range, 6mm aperture, 2cm -1 The standard transmission FTIR spectrum was obtained with a spectral resolution of 16 background scans, 16 spectral scans, an interferogram zero filling factor of 64 and Blackmann-Harris 3-term apodization. The spectrum corresponding to (CH2) was used. >2 The structural unit is 730cm -1 and 720cm -1 (A Q ) was used to quantitatively analyze the total area of CH2 rocking deformation at 762 cm -1 and 694cm -1 ). The quantitative band was normalized to 4323 cm -1 (A R ) corresponding to the CH band of the CH building block (integration method G, limit 4650 cm -1 ,4007cm-1). Then the secondary calibration curve was used to normalize the absorption (A Q / A R) predicts the ethylene content in weight percent. The calibration curve has been previously constructed by ordinary least squares (OLS) regression of the normalized absorbance and the main comonomer content measured on the calibration set.
[0209] Poly(propylene-co-ethylene)-ethylene content- 13 C NMR spectroscopy
[0210] A Bruker Avance III 400 NMR spectrometer was used to analyze the 1 H and 13 C to operate and record the quantity in solution state 13 C{ 1 H} NMR spectrum. Nitrogen was used for all atmospheres and the temperature was 125 °C. 13 All spectra were recorded with a 10 mm extended temperature probe optimized for C. About 200 mg of material was dissolved in 3 ml of 1,2-tetrachloroethane-d2 (TCE-d2) along with chromium(III) acetylacetonate (Cr(acac)3) to give a 65 mM solution of the relaxation agent in the solvent (Singh, G., Kothari, A., Gupta, V., Polymer Testing 285 (2009), 475).
[0211] To ensure a homogeneous solution, the NMR tube was further heated in a rotary furnace for at least 1 hour after initial sample preparation in a heating block. After insertion of the magnet, the tube rotated at 10 Hz. This setting was selected primarily for the quantitative needs required for high resolution and accurate quantification of ethylene content. Standard single pulse excitation was used in the absence of NOE, using an optimized vertex angle, 1 s recycle delay and a dual-level WALTZ16 decoupling scheme (Zhou, Z. et al., J. Mag. Reson., 187 (2007) 225, and Busico, V. et al., Macromol, Rapid Commun., 2007, 28, 1128). A total of 6144 (6k) transients were obtained for each spectrum. For quantitative 13 C{ 1 H} NMR spectra are processed, integrated, and the relevant quantitative properties are determined from the integration. All chemical shifts are indirectly referenced to the central methylene of the ethylene block (EEE) at 30.00 ppm using the chemical shift of the solvent. This method allows comparable references even when this structural unit is not present. Characteristic signals corresponding to ethylene incorporation are observed (Cheng, HN, Macromolecules 17 (1984), 1950), and the comonomer fraction is calculated as the fraction of ethylene in the polymer relative to all monomers in the polymer: fE = (E / (P+E)). Using the method of Wang et al., by13 C{ 1 The comonomer fraction is quantified by integrating multiple signals over the entire spectral region in the H} spectrum (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157). This method was chosen because of its accuracy and the ability to analyze the presence of regional defects when necessary. The integration area is slightly adjusted to increase applicability over the entire range of comonomer content encountered. For systems with very low ethylene content where only isolated ethylene is observed in the PPEPP sequence, the method of Wang et al. is modified to reduce the integral effect of sites that no longer exist. This method reduces the overestimation of the ethylene content of such systems and is achieved by reducing the number of sites used to determine the absolute ethylene content to E = 0.5 (Sββ + Sβγ + Sβδ + 0.5 (Sαβ + Sαγ)). By using this set of sites, using the same symbols used in the article by Wang et al., the corresponding integral equation becomes E = 0.5 (I H +I G +0.5(I C +I D ))(Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157). The equation for absolute propylene content was not modified. The mole percent of comonomer incorporation was calculated from the mole fraction: E [mol %] = 100 × fE. The weight percent of comonomer incorporation was calculated from the mole fraction: E [weight %] = 100 × (fE × 28.06) / ((fE × 28.06) + ((1-fE) × 42.08)).
[0212] f) Comonomer content
[0213] The comonomer content was determined using the film thickness method using the intensity of the dosing tape I(q) and the thickness T of the pressed film by the following relationship: [I(q) / T]m+c=C, where m and c are coefficients determined from a calibration curve using the coefficients given by 13 The comonomer content was constructed by C-NMR spectroscopy.
[0214] Based on 13 C-NMR calibrated Fourier transform infrared spectroscopy (FTIR) was used to measure the comonomer content in a known manner using a Nicolet Magna 550 IR spectrometer and Nicolet Omnic FTIR software. Films with a thickness of about 250 μm were compression molded from the samples. Similar films were prepared from calibration samples with known comonomer content. The comonomer content was determined by measuring the wavenumbers from 1430 to 1100 cm -1The absorbance is measured as the height of the peak by selecting the so-called short baseline or the long baseline or both. The short baseline is at about 1410-1320 cm -1 The long baseline is drawn at about 1410-1220 cm. -1 A specific calibration is required for each baseline type. In addition, the comonomer content of the unknown samples is within the range of the comonomer content of the calibration samples.
[0215] g) Talc and chalk content
[0216] TGA according to the following procedure:
[0217] Thermogravimetric analysis (TGA) experiments were performed using a Perkin Elmer TGA 8000. Approximately 10-20 mg of material was placed in a platinum pan. The temperature was equilibrated at 50°C for 10 minutes and then raised to 950°C at a heating rate of 20°C / min under nitrogen. The weight loss (WCO2) between 550°C and 700°C was attributed to CO2 released by CaCO3, and the chalk content was therefore estimated as:
[0218] Chalk content = 100 / 44×WCO2
[0219] The temperature was then reduced to 300°C at a cooling rate of 20°C / min. The gas was then switched to oxygen and the temperature was raised again to 900°C. The weight loss in this step was attributed to carbon black (Wcb). Knowing the contents of carbon black and chalk, the ash content excluding chalk and carbon black was calculated as follows:
[0220] Ash content = (ash residue) - 56 / 44 × WCO2 - Wcb
[0221] The ash residue is the weight % measured at 900° C. in a first step carried out under nitrogen. The ash content is estimated to be identical to the talc content of the regenerate studied.
[0222] h)MFR
[0223] The melt flow rate (MFR2) is measured at 230°C (polypropylene-based materials) or at 190°C (polyethylene-based materials) with a load of 2.16 kg. The melt flow rate is the amount of polymer in grams extruded in 10 minutes at a temperature of 230°C (or 190°C) according to a test device standardized according to ISO 1133 under a load of 2.16 kg.
[0224] i) Amount of metal
[0225] The amount of metal was determined by x-ray fluorescence (XRF).
[0226] j) Amount of paper and wood
[0227] Paper and wood were determined by conventional laboratory methods including grinding, flotation, microscopy and thermogravimetric analysis (TGA).
[0228] k) Limonene measurement
[0229] Limonene quantification was performed by standard addition using solid phase microextraction (HS-SPME-GC-MS).
[0230] 50mg of ground sample was weighed into a 20mL headspace vial, and after adding different concentrations of limonene and a glass-coated magnetic stirring bar, the vial was closed with a magnetic cap lined with silicone / PTFE. A known concentration of diluted limonene standard was added to the sample using a microcapillary (10pL). 0, 2, 20 and 100ng of addition was equal to 0mg / kg, 0.1mg / kg, 1mg / kg and 5mg / kg of limonene, and a standard amount of 6.6mg / kg, 11mg / kg and 16.5mg / kg of limonene was used in combination with some samples tested in this application. For quantification, ions-93 obtained in SIM mode were used. Enrichment of the volatile fraction was performed by headspace solid phase microextraction at 60°C with a 50 / 30pm DVB / Carboxen / PDMS fiber with a 2cm stable deflection for 20 minutes. Desorption was performed directly at 270°C in the heated injection port of the GCMS system.
[0231] GCMS parameters:
[0232] Column: 30m HP 5MS 0.25×0.25
[0233] Syringe: Splitless with 0.75 mm SPME liner, 270 °C
[0234] Temperature program: -10℃(1min)
[0235] Carrier gas: Helium 5.0, 31cm / s linear velocity, constant flow
[0236] MS: Single quadrupole, direct interface, 280°C interface temperature
[0237] Acquisition: SIM scan mode
[0238] Scan parameters: 20-300amu
[0239] SIM parameters: m / Z 93, 100 ms dwell time
[0240] l) Total free fatty acid content
[0241] Fatty acid quantification was performed by standard addition using headspace solid phase microextraction (HS-SPME-GC-MS).
[0242] 50mg grinding samples were weighed in 20mL headspace vials, and after adding different concentrations of limonene and glass-coated magnetic stirring bars, the vials were closed with magnetic caps lined with silicone / PTFE. Free fatty acid mixtures (acetic acid, propionic acid, butyric acid, valeric acid, caproic acid and octanoic acid) standards of known concentrations were added to the samples at three different levels using 10 μL microcapillaries. 0,50,100 and 500ng of addition were equal to each of 0mg / kg, 1mg / kg, 2mg / kg and 10mg / kg of each individual acid. For quantitative purposes, all acids except propionic acid (which uses ion 74) use ions 60 obtained in SIM mode.
[0243] GCMS parameters:
[0244] Column: 20m ZB wax plus 0.25×0.25
[0245] Syringe: With glass-lined splitter liner, 5:1 split, 250°C
[0246] Temperature program: 40℃ (1 minute) @6℃ / minute to 120℃, @15℃ to 245℃ (5 minutes)
[0247] Carrier: Helium 5.0, 40cm / s linear velocity, constant flow
[0248] MS: Single quadrupole, direct interface, 220°C interface temperature
[0249] Acquisition: SIM scan mode
[0250] Scan parameters: 46-250amu 6.6 scans / second
[0251] SIM parameters: m / z 60, 74, 6.6 scans / sec
[0252] m) Glass transition temperature
[0253] The glass transition temperatures of the iPP matrix and the elastomeric phase were determined by dynamic mechanical thermal analysis according to ISO 6721-7. Compression molded samples (40×10×1 mm2) were subjected to 100 % calorimetric analysis using a TA Ares G2 testing apparatus in torsional deformation mode at a heating rate of 2°C / min and a frequency of 1 Hz between −130°C and +160°C. 3 ) for measurement.
[0254] n) VOC content
[0255] The VOC content is determined in accordance with VDA 278 on compositions obtained directly from compounding, ie only storage as described in VDA 278 has taken place.
[0256] o) Particle size distribution of fillers, especially talc
[0257] Median particle size d 50 and top cut particle size d 95 Measured by gravimetric liquid sedimentation according to ISO 13317-3.
[0258] p) Xylene solubles (XCS, wt%):
[0259] The xylene cold soluble (XCS) content is determined according to ISO 16152, first edition, 2005-07-01 at 25° C. The part that remains insoluble is the xylene cold insoluble (XCI) fraction.
[0260] q) Intrinsic viscosity
[0261] The intrinsic viscosity is measured according to DIN ISO 1628 / 1, October 1999 (in decalin at 135° C.).
[0262] r) Ash content
[0263] Ash content is measured according to ISO 3451-1 (1997) standard.
[0264] s) Density
[0265] Density was measured according to ISO 1183-187. Sample preparation was performed by compression molding according to ISO 1872-2:2007.
[0266] t) Heat deflection temperature (HDT):
[0267] HDT was prepared in accordance with ISO 1873-2 in 80×10×4 mm 3 The test is carried out according to ISO 75, condition A, on flat supported specimens with a nominal surface stress of 1.80 MPa.
[0268] u)DSC analysis, melting temperature (Tm) and heat of fusion (Hf), crystallization temperature (Tc) and melting enthalpy (Hm):
[0269] All DSC parameters were measured with a TA Instrument Q200 differential scanning calorimetry (DSC) on 5 to 7 mg samples. DSC was run in a heating / cooling / heating cycle at a scan rate of 10°C / min in the temperature range of -30 to +225°C according to ISO 11357 / Part 3 / Method C2. The crystallization temperature (Tc) was determined by the cooling step, while the melting temperature (Tm) and the melting enthalpy (Hm) were determined by the second heating step. The crystallinity was calculated from the melting enthalpy by assuming a Hm value of 209 J / g for fully crystalline polypropylene (see Brandrup, J., Immergut, EH, Eds., Polymer Handbook, 3rd edition, Wiley, New York, 1989; Chapter 3).
[0270] v) Paint Adhesion:
[0271] Adhesion is characterized by the resistance of a decorative coating such as paint when subjected to high pressure cleaning washing under certain conditions as described below.
[0272] To measure the coating adhesion of the compositions, injection molded sample plaques (150 mm x 80 mm x 3 mm) were produced at a melt temperature of 240°C and a mold temperature of 50°C. The flow front speed was 100 mm / s. Prior to coating, the Zeller Gmelin The plate was cleaned at 1000 mm / s for 5 minutes. Subsequently, the surface was activated by combustion, wherein a mixture of propane (9 l / min) and air (180 l / min) in a ratio of 1:20 was spread over the polymer substrate with a burner at a speed of 670 mm / s. The polymer substrate was then coated with 3 layers (i.e. a primer, a topcoat (black) and a varnish). The combustion step was performed twice.
[0273] The decorative coating is cut down to the substrate to a total depth of about 500 μm (including coating and substrate) with a cutting tool forming a cross with 100 mm long branches. On each coated substrate, 3 lines with corresponding crosses are cut. The cut area is further exposed to hot water vapor at a temperature T, which is directed to the surface of the test panel at a distance d and at an angle α for a duration t. The pressure of the water jet is generated by the flow rate of the water and is determined by the type of nozzle installed at the end of the water pipe.
[0274] Use the following parameters:
[0275] T(water)=68°C; t=30 seconds; d=100 mm, α=90°, water pressure 65 bar, nozzle type=Walter 13 / 32.
[0276] By quantifying each test line in mm 2Adhesion was evaluated by measuring the failed or delaminated coating area. For each example, 5 panels (150 mm × 80 mm × 3 mm) were tested. For this purpose, images of the test lines were taken before and after steam jet exposure. The delamination area was then calculated using image processing software. The average failure area of 3 test lines on 5 test samples (i.e., the average of a total of 15 test points) was reported as the average failure area. SD is the standard deviation, which is determined according to the following formula:
[0277]
[0278] in:
[0279] x is the observed value;
[0280] is the mean of the observations; and
[0281] n is the number of observations.
[0282] experiment
[0283] Catalyst system:
[0284] For the polymerization process of HECO 1 and HECO 2, a conventional transesterified high yield MgCl2 supported Ziegler-Natta polypropylene catalyst component containing diethyl phthalate as an internal donor was used. Triethylaluminum (TEAL) was used as a cocatalyst, and dicyclopentyldimethoxysilane (D-donor) was used as an external donor. Catalyst components and their preparation concepts are generally described in, for example, patent publications EP491566, EP591224 and EP586390.
[0285] Therefore, the catalyst component is prepared as follows: first, under inert conditions, 0.1mol MgCl2×3EtOH is suspended in 250ml decane in a normal pressure reactor. The solution is cooled to -15°C and 300ml cold TiCl4 is added while the temperature is maintained at the temperature. Then, the temperature of the slurry is slowly raised to 20°C. At this temperature, 0.02mol dioctyl phthalate (DOP) is added to the slurry. After the addition of phthalate, the temperature is raised to 135°C during 90 minutes and the slurry is allowed to stand for 60 minutes. Then, another 300ml of TiCl4 is added, and the temperature is maintained at 135°C for 120 minutes. Afterwards, the catalyst is filtered from the liquid and washed 6 times with 300ml heptane at 80°C. Then, the solid catalyst component is filtered and dried.
[0286] HECO 1 and HECO 2 were prepared in a prepolymerization / loop reactor / gas phase reactor 1 / gas phase reactor 2 / gas phase reactor 3 configuration followed by a pelletizing step. The catalyst system defined above was used in combination with dicyclopentadienyl-dimethoxysilane (donor D) as external donor.
[0287] Table 1: Preparation of HECO 1 and HECO 2
[0288]
[0289]
[0290]
[0291] The heterophasic copolymers HECO1 and HECO2 were mixed at 220°C in a co-rotating twin-screw extruder Coperion ZSK 47 with 0.15 wt% of antioxidant (Irganox B215FF from BASF AG, Germany, a 1:2 mixture of pentaerythritol-tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)-propionate (CAS-no. 6683-19-8) and tris(2,4-di-tert-butylphenyl)phosphite (CAS-no. 31570-04-4); 0.05 wt% of calcium stearate (CAS-no. 1592-23-0, commercially available from Faci, Italy).
[0292] Table 2 shows the properties of the polypropylene / polyethylene blends (A) used for evaluation.
[0293] Table 2: Properties of polypropylene / polyethylene blends (blend A)
[0294]
[0295] Table 3: Comparison of basic properties of HECO1 and HECO2 with blends (A).
[0296]
[0297]
[0298] As can be seen from Table 3, the replacement of HECO1 and / or HECO2 by blend (A) is not foreseeable.
[0299] The final composition was compounded in a Coperin ZSK40 twin screw extruder at 220°C using the polymer prepared by recycling as described above and talc Jetfine 3CA (d 50 =1.2μm; d 95=3.3μm), antioxidant, UV stabilizer, slip agent, nucleating agent, carbon black masterbatch, calcium stearate, antifogging agent.
[0300]
[0301]
[0302] *Paintability test, average delamination area
[0303] As can be seen, for all inventive examples, the impact strength, in particular the Charpy impact at 23°C, is surprisingly improved. Moreover, for inventive examples IE2 and IE3, the low temperature impact is also surprisingly kept at a comparable level, at a slightly lower level. These improvements can be obtained at a stiffness loss of about 150 MPa to about 350 MPa. Thus, for automotive applications that do not have too high stiffness requirements, surprisingly high substitution of HECO1 and HECO2 is possible. Inventive examples IE1 and IE2 both include an amount of 25 wt% of the regenerant "Blend A", which also has a surprisingly high HDT (ISO 75B) very close to the comparative example CE1 that does not include any regenerant. Reference example RE2 (not within the scope of the claims) shows that a complete replacement of HECO1 is conceivable, but the stiffness is too low. Inventive example IE3 shows that the amount of regenerant can be further increased with surprisingly little deterioration of the overall melt flow rate and stiffness. All inventive examples also show similar anisotropy when the temperature is increased from 23°C to 80°C.
Claims
1. A composition suitable for automotive applications, in, The composition By blending at least components a) to f) obtain: a) 5.0 to 45 wt% of a first heterophasic polypropylene copolymer HECO 1, b) 2.0 to 20 wt% of a second heterophasic polypropylene copolymer HECO 2, c) 10 to 60 wt% of a polypropylene-polyethylene blend A, d) 2.5 to 25 wt% of an ethylene elastomer, e) 5.0 to 30 wt% of an inorganic filler, f) 0.1 to 4.0 wt% of additives, wherein all percentages refer to the total composition, and (i) the first heterophasic polypropylene copolymer HECO 1 comprises a matrix phase and an elastomeric phase dispersed therein, the first heterophasic polypropylene copolymer HECO 1 having: - Melt flow rate MFR measured at 230°C according to ISO 1133 2 75 to 200 g / 10 min; - the xylene cold soluble fraction XCS has an intrinsic viscosity of 1.2 to 3.2 dl / g, measured in decalin at 135° C. according to DIN ISO 1628 / 1; and (ii) the second heterophasic polypropylene copolymer HECO 2 comprises a matrix phase and an elastomeric phase dispersed therein, the second heterophasic polypropylene copolymer HECO 2 having: - Melt flow rate MFR measured at 230°C according to ISO 1133 2 2.5 to 10 g / 10 min; and - the xylene cold soluble fraction XCS has an intrinsic viscosity of 4.0 dl / g to 10 dl / g, measured in decalin at 135° C. according to DIN ISO 1628 / 1; (iii) Polypropylene-polyethylene blend A comprises: A-1) Polypropylene, A-2) Polyethylene, The weight ratio of polypropylene to polyethylene is 19:1 to 7:3, and the polypropylene-polyethylene blend A has: - Melt flow rate MFR measured at 230°C according to ISO 1133 2 5.0 to 30 g / 10 min; - a xylene cold soluble fraction XCS, measured at 25°C according to ISO 16152, first edition, of 2.0 to 15 wt%; - Optionally, a residual ash content of less than 3.0 wt%, and The polypropylene-polyethylene blend A has one or more of the following characteristics: (aa) a limonene content of 0.1 ppm to 100 ppm as determined by headspace solid phase microextraction coupled to gas chromatography and mass spectrometry; (bb) a fatty acid content of 0.1 to 100 ppm as determined by headspace solid phase microextraction coupled to gas chromatography and mass spectrometry; as well as - the ethylene-based elastomer is selected from C2C4 elastomers, C2C6 elastomers and / or C2C8 elastomers, and the ethylene-based elastomer: - having a melt flow rate MFR of 0.05 to 5.0 g / 10 min measured at 190° C. according to ISO 1133 2 , -With 850 to 885 kg / m 3 density; and (iv) inorganic fillers, -Has a median particle size d of 0.3 to 3.0 microns before compounding 50 ; The total amount of components a) to e) is at least 90 wt % of the composition suitable for automotive applications.
2. The composition suitable for automotive applications according to claim 1, in, The composition By blending at least components a) to f) obtain: a) 5.0 to 45 wt% of a first heterophasic polypropylene copolymer HECO 1, b) 2.0 to 20 wt% of a second heterophasic polypropylene copolymer HECO 2, c) 10 to 60 wt% of a polypropylene-polyethylene blend A, d) 2.5 to 25 wt% of an ethylene elastomer, e) 5.0 to 30 wt% of an inorganic filler, f) 0.1 to 4.0 wt% of additives, wherein all percentages refer to the total composition, wherein, (ee) the first heterophasic polypropylene copolymer HECO 1 comprises a matrix phase and an elastomeric phase dispersed therein, the first heterophasic polypropylene copolymer HECO 1 having: - Melt flow rate MFR measured at 230°C according to ISO 1133 2 75 to 200 g / 10 min; - a xylene cold soluble fraction XCS, measured at 25°C according to ISO 16152, first edition, of 8.0 to 20.0 wt%; - the intrinsic viscosity of the xylene cold soluble fraction XCS, measured in decalin at 135° C. according to DIN ISO 1628 / 1, is from 1.2 dl / g to 3.2 dl / g; - Melt flow rate MFR of the xylene insoluble XCI fraction measured at 230°C according to ISO 1133, determined at 25°C according to the first edition of ISO 16152 2 100 to 500 g / 10 min, - a content of units derived from ethylene in the xylene cold soluble fraction XCS of 25.0 to 50.0 wt %, - a total content of units derived from ethylene of from 2.0 to 13.0 wt.%; (ff) the second heterophasic polypropylene copolymer HECO 2 comprises a matrix phase and an elastomeric phase dispersed therein, the second heterophasic polypropylene copolymer HECO 2 having: - Melt flow rate MFR measured at 230°C according to ISO 1133 2 2.5 to 10 g / 10 min; - a xylene cold soluble fraction XCS, measured at 25°C according to ISO 16152, first edition, of 20 to 50 wt%; - the xylene cold soluble fraction XCS has an intrinsic viscosity of 4.0 to 10 dl / g, measured in decalin at 135° C. according to DIN ISO 1628 / 1; and - Melt flow rate MFR of the xylene insoluble XCI fraction measured at 230°C according to ISO 1133, determined at 25°C according to the first edition of ISO 16152 2 20 to 90 g / 10 min, - the content of units derived from ethylene in the xylene cold soluble fraction XCS is from 15.0 to 25.0 wt %, The total content of units derived from ethylene is from 3.0 to 15.0 wt %, and (gg) Polypropylene-polyethylene blend A comprises: A-1) Polypropylene, A-2) Polyethylene, The weight ratio of polypropylene to polyethylene is 19:1 to 7:3, and the polypropylene-polyethylene blend A has: - Melt flow rate MFR measured at 230°C according to ISO 1133 2 5.0 to 30 g / 10 min; - a xylene cold soluble fraction XCS, measured at 25°C according to ISO 16152, first edition, of 2.0 to 15 wt%; and - Optionally, the residual ash content is less than 3.0 wt%, The polypropylene-polyethylene blend A has one or more of the following characteristics: (aa) a limonene content of 0.1 ppm to 100 ppm as determined by headspace solid phase microextraction coupled to gas chromatography and mass spectrometry; (bb) a fatty acid content of 0.1 to 100 ppm as determined by headspace solid phase microextraction coupled to gas chromatography and mass spectrometry; (cc) a polyamide content of 0.05 to 1.5 wt % as determined by NMR; (dd) a polystyrene content of 0.05-3.0 wt % as determined by NMR; as well as -The ethylene-based elastomer is selected from C2C4 elastomer, C2C6 elastomer and / or C2C8 elastomer, wherein: - having a melt flow rate MFR of 0.05 to 5.0 g / 10 min measured at 190° C. according to ISO 1133 2 , -With 850 to 885 kg / m 3 density; and (ee) Inorganic filler: -Has a median particle size d of 0.3 to 3.0 microns before compounding 50 ; -and The total amount of components a) to e) is at least 90 wt % of the composition suitable for automotive applications.
3. A composition suitable for automotive applications according to claim 1 or 2, in, The composition has a tensile modulus measured at 23° C. according to ISO 527.2 of 1300 MPa to 1700 MPa.
4. A composition suitable for automotive applications according to claim 1 or 2, in, The composition is obtained by blending at least components a) to f), a) 20 to 35 wt% of a first heterophasic polypropylene copolymer HECO 1, b) 5.0 to 20 wt% of a second heterophasic polypropylene copolymer HECO 2, c) 20 to 30 wt% of a polypropylene-polyethylene blend A, d) 7.0 to 22 wt% of an ethylene elastomer, e) 5.0 to 25 wt% of an inorganic filler, f) 0.1 to 4.0 wt% of additives.
5. The composition according to claim 4, suitable for automotive applications, in, The composition has a tensile modulus of 1400 MPa to 1700 MPa measured at 23° C. according to ISO 527.2, and Having a thermal conductivity of at least 40 kJ / m2 measured in non-instrumented mode at +23 °C according to ISO 179-1eA 2 Charpy notched impact strength.
6. The composition suitable for automotive applications according to claim 4, in, The composition has a heat deflection temperature of at least 90°C as measured according to ISO 75B.
7. A composition suitable for automotive applications according to claim 1 or 2, in, The composition has a melt flow rate of 10.0 to 25 g / 10 min, measured at 230° C. with a load of 2.16 kg according to ISO 1133.
8. A composition suitable for automotive applications according to claim 1 or 2, in, The composition can be obtained by blending at least components a) to f), a) 5.0 to 20 wt% of a first heterophasic polypropylene copolymer HECO 1, b) 2.5 to 7.0 wt% of a second heterophasic polypropylene copolymer HECO 2, c) 30 to 55 wt% of a polypropylene-polyethylene blend A, d) 7.0 to 22 wt% of an ethylene elastomer, e) 5.0 to 25 wt% of an inorganic filler, f) 0.1 to 4.0 wt% of additives.
9. The composition suitable for automotive applications according to claim 8, in, The composition having a tensile modulus of 1200 to 1400 MPa measured at 23°C according to ISO 527.2, and Having a thermal conductivity of at least 40 kJ / m2 measured in non-instrumented mode at +23 °C according to ISO 179-1eA 2 Charpy notched impact strength.
10. The composition suitable for automotive applications according to claim 8, in, The composition has a melt flow rate of 6.0 to 15 g / 10 min, measured at 230° C. with a load of 2.16 kg according to ISO 1133.
11. The composition suitable for automotive applications according to claim 1 or 2, wherein the additive is selected from one or more of an antioxidant, a UV stabilizer, a slip agent, a nucleating agent, a pigment, a lubricant, a masterbatch polymer and / or an antifogging agent.
12. A composition suitable for automotive applications according to claim 1 or 2, in, The composition has a VOC of less than 75 μg / g of composition, the VOC being measured on material directly obtained by extrusion according to the process as described in VDA 278.
13. A composition suitable for automotive applications according to claim 1 or 2, in, The coating adhesion of the composition is less than 24 mm 2 , the coating adhesion is evaluated in mm 2 The measured coating area is the area of failure or delamination.
14. An article comprising the composition of any one of claims 1 to 13.