Titanium surface treatment methods

Through a multi-step titanium surface treatment method, including acid solution etching, ultrasonic treatment and silane coupling treatment, fine cracks and oxide films are formed, which solves the problem of low bonding strength between polymer and titanium, significantly improves binding strength and sealing, and reduces the bonding strength and strength. Component weight and cost.

CN116136023BActive Publication Date: 2024-11-15DONGGUAN DSP TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211435646.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-16
Filing Date
2022-11-16
Publication Date
2024-11-15
Estimated Expiration
2042-11-16

AI Technical Summary

Technical Problem

The low bonding strength between polymer and titanium leads to the reliability of the polymer-titanium bonding structure. It is difficult for existing anodizing treatment methods to effectively improve the bonding strength and friction.

Method used

Multi-step titanium surface treatment method is adopted, including acid solution etching, ultrasonic treatment, silane coupling treatment and anodization, and the binding force of the titanium surface to the polymer is enhanced by forming fine cracks and oxide films.

Benefits of technology

The bonding strength and sealing between polymer and titanium are significantly improved, the service life of the components is extended, and the weight and production costs are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116136023B_ABST
    Figure CN116136023B_ABST
Patent Text Reader

Abstract

The present invention provides a titanium surface treatment method for manufacturing a polymer-titanium bonding structure with excellent bonding strength. The titanium surface treatment method for bonding with a polymer composite material comprises: (a) a first etching step, wherein the titanium surface is etched with an acidic solution; (b) a first surface treatment step, wherein the titanium surface is ultrasonically treated; (c) a second etching step, wherein the titanium surface is etched again with an acidic solution; (d) a second surface treatment step, wherein the titanium surface is ultrasonically treated again; (e) a first silane coupling treatment step, wherein the titanium surface is ultrasonically treated; (f) a third surface treatment step, wherein the titanium surface is ultrasonically treated again; (g) a second silane coupling treatment step, wherein the titanium surface is anodized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a titanium surface treatment method, in particular to a titanium surface treatment method for bonding a polymer-titanium bonding structure, wherein the bonding between the titanium surface and the polymer is maximized through primary and secondary silane coupling treatment of the titanium surface. Background Art

[0002] Although polymer-titanium bonded structures are widely used in automotive and electronic parts and assemblies, low reliability of the bonding strength between polymer and titanium has been recognized as a problem.

[0003] At the same time, the titanium surface is treated by anodizing to increase the activity and friction of the titanium surface and form a strong bond with the polymer. Summary of the invention

[0004] [Technical Problems to be Solved by the Invention]

[0005] The present invention aims to solve the above technical problems and provides a titanium surface treatment method for manufacturing a polymer-titanium bonding structure with excellent bonding strength.

[0006]

Technical means to solve technical problems

[0007] A titanium surface treatment method for bonding with a polymer composite material, comprising:

[0008] (a) a first etching step, wherein the titanium surface is etched with an acidic solution;

[0009] (b) a first surface treatment step, wherein the titanium surface is subjected to ultrasonic treatment;

[0010] (c) a second etching step, wherein the titanium surface is etched again with an acidic solution;

[0011] (d) a second surface treatment step, wherein the titanium surface is again subjected to ultrasonic treatment;

[0012] (e) a first silane coupling treatment step, wherein the titanium surface is subjected to ultrasonic treatment;

[0013] (f) a third surface treatment step, wherein the titanium surface is again subjected to ultrasonic treatment;

[0014] (g) A second silane coupling treatment step, wherein the titanium surface is subjected to anodization treatment.

[0015] The titanium surface treatment method of the present invention as described above comprises:

[0016] In the step (e), ultrasonic treatment is performed for 10-300 seconds at 30-70° C. with an output of 400 W and a frequency of 24-100 kHz in a solution containing 10-50 wt % of an alkaline solution and 0.1-1 wt % of a first silane coupling agent, wherein in the alkaline solution, caustic soda (concentration of 1-10%), sodium carbonate (concentration of 1-10%) and ammonium nitrate (concentration of 1-10%) are mixed in a ratio of 3:1:1.

[0017] The titanium surface treatment method of the present invention as described above comprises:

[0018] The step (f) is carried out in an acidic solution containing a mixture of at least two or more of sulfuric acid (with a concentration of 1-10%), phosphoric acid (with a concentration of 1-10%) and nitric acid (with a concentration of 1-10%) or in an alkaline solution containing a mixture of at least two or more of alkalis including caustic soda (with a concentration of 1-10%), sodium carbonate (with a concentration of 1-10%) and ammonium nitrate (with a concentration of 1-10%), at 30-70° C. with an ultrasonic treatment having an output of 400 W and a frequency of 24-100 kHz for 10-300 seconds;

[0019] The titanium surface treatment method of the present invention as described above comprises:

[0020] Step (g) in a solution containing 10-50 wt.% of an electrolyte solution and 0.1-1 wt.% of a second silane coupling agent, using a rectifier at 30-70°C and at 0.1-10 A / dm 2 The process is carried out for 1-30 minutes with a current density of 500 ms and a positive pulse duration (application time), wherein in the electrolyte solution, NaOH, KOH, Ca(OH)2 and NaHCO3 are mixed in a ratio of 3:1:1:1.

[0021] The titanium surface treatment method of the present invention as described above comprises:

[0022] The silane coupling agent is (RO)3Si-(CH2)3-NH2, (RO)3Si-(CH2)2-Si(OC2H5)3, (RO)3Si-(CH2)3-SH, (RO)3Si-CH=CH2, (RO)3Si-(CH3)3-OOC(CH3)C=CH2, (RO)3Si-(CH3)3-O-CHCH2O and (RO)3Si-(CH2) 15 A mixture of at least two or more of CH3.

[0023] The titanium surface treatment method of the present invention as described above comprises:

[0024] The first silane coupling agent and the second silane coupling agent are a mixture of different types.

[0025]

Beneficial technical effects

[0026] The titanium alloy surface is etched with an acid solution to roughen the titanium alloy surface, and the surface is roughened together with microcracks by a primary surface treatment with ultrasonic waves.

[0027] Then, through primary and secondary silane coupling treatments using ultrasonic waves, a large number of fine cracks are formed on the surface, and the silane coupling agent penetrates into the generated cracks to maximize the bonding force between the polymer and titanium. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The surface changes according to each process of titanium surface treatment are shown;

[0029] Figure 2A-2B Shows Figure 1 Cross-sectional photograph of the final titanium surface;

[0030] Figure 3 An ultrasonic device is shown;

[0031] Figure 4 shows the anodizing apparatus and conditions;

[0032] In Figure 5, Figure 5A The conventional product and the titanium sample of the present invention are shown. Figure 5B The conventional product and the samples of the present invention combined with each polymer are shown. Figure 5C The tensile test method of the conventional product and the product of the present invention after each constant temperature and humidity test is shown;

[0033] Figure 6 The tensile test results of the conventional product and the product of the present invention after constant temperature and humidity testing are shown respectively;

[0034] Figure 7 Photographs showing fracture surfaces of tensile tests of conventional products and the product of the present invention after each constant temperature and humidity test;

[0035] Figure 8 A comparison diagram of each independent time (neglect time) of the tensile test between the conventional product and the present invention is shown;

[0036] FIG9 shows a constant temperature and humidity test measuring machine and a test piece;

[0037] Fig.10 A comparison chart of the constant temperature and humidity test results of the conventional product and the product of the present invention is shown. DETAILED DESCRIPTION

[0038] The method for manufacturing the polymer titanium bonding structure is described below with reference to the accompanying drawings.

[0039] A method for treating a titanium surface for bonding to a polymer composite material, comprising:

[0040] (a) a first etching step, wherein the titanium surface is etched with an acidic solution;

[0041] (b) a first surface treatment step, wherein the titanium surface is treated with ultrasound;

[0042] (c) a second etching step, wherein the titanium surface is etched again with an acidic solution;

[0043] (d) a second surface treatment step, wherein the titanium surface is again subjected to ultrasonic treatment;

[0044] (e) a first silane coupling treatment step, wherein the titanium surface is subjected to ultrasonic treatment;

[0045] (f) a third surface treatment step, wherein the titanium surface is again subjected to ultrasonic treatment;

[0046] (g) A second silane coupling treatment step, wherein the titanium surface is subjected to anodization treatment.

[0047] In step (a), a first etching treatment is carried out in an acidic solution containing typically sulfuric acid, phosphoric acid and a trace amount of nitric acid at 30-60° C. for 10-300 seconds.

[0048] In the first etching step, etching traces are formed on the titanium surface, and the titanium surface becomes rough.

[0049] In step (b), the first surface treatment using ultrasonic waves is performed in a general alkaline solution at 30-60° C. and an output of 400 W at a frequency of 24-100 kHz for 10-300 seconds.

[0050] Micro cracks are formed on the titanium surface etched by the first surface treatment.

[0051] In step (c), a second etching treatment is performed in an acidic solution containing typically sulfuric acid, phosphoric acid and a trace amount of nitric acid at 30-60° C. for 10-300 seconds.

[0052] In the second etching step, further etching marks are formed on the titanium surface, and the titanium surface becomes rougher.

[0053] In step (d), the second surface treatment using ultrasound is performed in a general alkaline solution at 30-60° C. and an output of 400 W at a frequency of 24-100 kHz for 10-300 seconds.

[0054] Further micro cracks are formed on the titanium surface etched by the first surface treatment.

[0055] In step (e), the first silane coupling treatment is carried out in a solution containing 10-50wt.% alkaline solution and 0.1-1wt.% of the first silane coupling agent, at 30-70°C, with an ultrasonic treatment of 400W output and 24-100kHz frequency for 10-300 seconds, wherein in the alkaline solution, caustic soda (concentration of 1-10%), sodium carbonate (concentration of 1-10%) and ammonium nitrate (concentration of 1-10%) are mixed in a ratio of 3:1:1.

[0056] Microcracks are further formed on the etched titanium surface, and the silane coupling agent is allowed to penetrate into the formed microcracks.

[0057] In step (e), the first silane coupling agent is (RO)3Si-(CH2)3-NH2, (RO)3Si-(CH2)2-Si(OC2H5)3, (RO)3Si-(CH2)3-SH, (RO)3Si-CH=CH2, (RO)3Si-(CH3)3-OOC(CH3)C=CH2, (RO)3Si-(CH3)3-O-CHCH2O and (RO)3Si-(CH2) 15 A mixture of at least two or more of CH3.

[0058] In step (f), the third surface treatment using ultrasound is carried out in an acidic solution containing a mixture of at least two or more of sulfuric acid (concentration of 1-10%), phosphoric acid (concentration of 1-10%) and nitric acid (concentration of 1-10%) or in an alkaline solution containing a mixture of at least two or more of caustic soda (concentration of 1-10%), sodium carbonate (concentration of 1-10%) and ammonium nitrate (concentration of 1-10%), at 30-70° C., with ultrasound treatment at a frequency of 24-200 kHz and an output of 400 W for 10-300 seconds.

[0059] The roughness of the titanium surface was roughened by etching and ultrasonic waves, and about 60% of the first silane coupling agent that had penetrated into the titanium surface was removed.

[0060] In step (g), the second silane coupling treatment is carried out in a solution containing 10-50 wt.% of an electrolyte solution and 0.1-1 wt.% of a second silane coupling agent, using a rectifier at 30-70°C, a positive duration (application time) of a 500 ms pulse, and a current of 0.1-10 A / dm 2 The electrolyte solution is treated at a current density of 1 to 30 minutes; wherein, NaOH, KOH, Ca(OH)2 and NaHCO3 are mixed in a ratio of 3:1:1:1.

[0061] This step forms a nano-thin sheet oxide film on the titanium surface. The second silane coupling agent, which is different from the first silane coupling agent, further penetrates the microcracks on the titanium surface and has a strong bonding force between the titanium surface and the polymer.

[0062] In step (g), the second silane coupling agent is (RO)3Si-(CH2)3-NH2, (RO)3Si-(CH2)2-Si(OC2H5)3, (RO)3Si-(CH2)3-SH, (RO)3Si-CH=CH2, (RO)3Si-(CH3)3-OOC(CH3)C=CH2, (RO)3Si-(CH3)3-O-CHCH2O and (RO)3Si-(CH2) 15 A mixture of at least two or more of CH3.

[0063] The second silane coupling agent in step (g) is a mixture of a different type from the first silane coupling agent in step (e).

[0064] Through different silane coupling agents, the bonding between the titanium surface and the polymer is stronger.

[0065] After the second silane coupling treatment, oxidation occurs through fine microcracks generated in the oxide film protrusions on the titanium surface, and additional fine oxide film protrusions are generated from the microcracks. Therefore, the contact area on the titanium surface is maximized, thereby maximizing the bonding force between titanium and the polymer. In addition, a bonding superposition force is generated between the additive remaining in the anodized titanium oxide film and the polymer to form an additional bonding force.

[0066] Figure 1 The structure and changes of the titanium alloy surface produced by various processes of titanium alloy surface treatment are shown.

[0067] Figure 2A Detailed image of the titanium surface after the final surface treatment process is shown in FIG.

[0068] As shown in the figure, the thickness of the oxide film such as microcracks and snowflakes infiltrated with silane coupling agent is 10-500nm.

[0069] Figure 2B A cross-sectional photograph of a titanium surface after the final surface treatment process is shown in FIG.

[0070] The formation of oxide coatings such as microcracks and nanosheets could be confirmed.

[0071] Specific embodiments and drawings are described below.

[0072] In order to demonstrate the effect of the present invention, experiments were conducted by making 10 test pieces for each of the conventional embodiment and embodiments 1-3.

[0073] As the usable titanium metal, titanium alloys ranging from Ti-1 grade to Ti-23 grade can be used.

[0074] The samples used in the experiment were Ti-2 grade titanium alloy specimens.

[0075] The composition of Ti-2 grade is shown in Table 1 below:

[0076] Table 1

[0077] N C H Fe O Ti 0.03% 0.08% 0.015% 0.3% 0.25% Bal.

[0078] The polymers that can be used in the present invention are composite resins, polyethylene, polypropylene, polyvinyl chloride, polyvinyl acetate, polyacrylate, polymethacrylate, unsaturated polymers, polyamide, polyether, polystyrene, polyester, and polyphenylene ether, polyphenylene sulfide, polybutadiene, polybutylene terephthalate, polymethylpentene, liquid crystal polymers, etc.

[0079] Table 2

[0080]

[0081] [Conventional Embodiment]

[0082] After step (a) to step (d), a sample is prepared by a conventional method. The conventional method is to use a 500 ms pulse rectifier at 50°C, 5 A / dm 2 The treatment was carried out for 15 minutes at a current density of 500 ms with a forward duration (application time), wherein in the electrolyte solution, NaOH, KOH, Ca(OH)2 and NaHCO3 were mixed in a ratio of 3:1:1:1.

[0083] [Example 1]

[0084] After steps (a) to (d), a sample is prepared by the method of the present invention. In step (e), a first silane coupling treatment is performed in a solution containing 25 wt.% of an alkaline solution and 0.5 wt.% of a first silane coupling agent (a mixture of (RO)3Si-(CH2)2-Si(OC2H5)3 and (RO)3Si-(CH2)3-SH in a mixing ratio of 1:3), at 30-70°C, with an output of 400 W and a frequency of 60 kHz for 150 seconds, wherein in the alkaline solution, caustic soda (concentration of 5%), sodium carbonate (concentration of 5%) and ammonium nitrate (concentration of 5%) are mixed in a ratio of 3:1:1.

[0085] [Example 2]

[0086] After steps (a) to (e), a sample is prepared by the method of the present invention. In step (f), a third surface treatment using ultrasound is performed in an acidic solution containing a mixture of sulfuric acid (concentration is 5%) and phosphoric acid (concentration is 5%) at 50° C., with an ultrasound treatment frequency of 60 kHz and an output of 400 W for 150 seconds.

[0087] [Example 3]

[0088] After steps (a) to (f), a sample is prepared by the method of the present invention. In step (g), in a solution containing 25 wt.% of an electrolyte solution and 0.5 wt.% of a second silane coupling agent (a mixture of (RO)3Si-(CH2)3-NH2 and (RO)3Si-(CH2)2-Si(OC2H5)3 in a mixing ratio of 3:1), a rectifier is used at 50°C, a positive duration (application time) of a 500 ms pulse, and a current of 5 A / dm 2 The second silane coupling treatment was performed with a current density of 15 minutes, wherein in the electrolyte solution, NaOH, KOH, Ca(OH)2 and NaHCO3 were mixed in a ratio of 3:1:1:1.

[0089] For the conventional embodiment and embodiments 1-3, the following resistance value measurement, T-bend test, tensile test, coupling force measurement and sealing experiment based on placement time were respectively performed. The results are as follows.

[0090]

Test 1

[0091] The samples used in the conventional examples and examples 1-3 were as follows Figure 5A The Ti-2 grade titanium alloy shown has a width of 12 mm, a length of 20 mm, a thickness of 3 mm, and Figure 5B As shown, titanium samples produced by the processes of the conventional embodiment and embodiments 1-3 are longitudinally combined.

[0092] As shown in Figure 5, in order to measure the bonding strength, tensile tests were performed before and after 1000 hours of constant temperature and humidity. The results are as follows: Figure 6 shown.

[0093] Figure 5A shows the test specimens manufactured for the tensile test, Figure 5B A polymer was superimposed on the titanium test piece of each embodiment.

[0094] Figure 5C Photographs showing the tensile testing method.

[0095] like Figure 6As shown in the curve graph, it can be seen that the sample of Example 1 has better tensile force than the sample of the traditional example before / after the constant temperature and humidity test.

[0096] Furthermore, it can be seen that the sample of Example 2 has better tensile strength than the sample of Example 1 before / after the constant temperature and humidity test.

[0097] Finally, it can be seen that, relative to the sample of Example 2, the sample of Example 3 has the best tensile force before / after the constant temperature and humidity test.

[0098] Figure 7 Photographs showing the amount of polymer remaining on the separated titanium surfaces of the test pieces of the conventional example and Examples 1-3 after the tensile test was completed after the constant temperature and humidity test.

[0099] As for the separated surface of the sample of the conventional example, it was easily separated, and it can be seen that the amount of the polymer on the titanium surface after separation was about 30%.

[0100] From the photograph of the separated surface of the sample of Example 1, it can be seen that the amount of polymer on the titanium surface after separation is about 40%.

[0101] From the photograph of the separated surface of the test piece of Example 2, it can be seen that the amount of polymer on the titanium surface after separation is about 50%.

[0102] From the photograph of the separated surface of the test piece of Example 3, it can be seen that the amount of polymer on the titanium surface after separation is about 80%.

[0103] Figure 8 The tensile strength test results of the test samples varying with time from 1 month to 12 months after polymer superposition are shown.

[0104] Thus, it can be seen that the specimen of Example 1 is superior to the specimen of the conventional embodiment in terms of the decrease in tension caused by the passage of time.

[0105] In addition, it can be seen that as time goes by, the tensile force of Example 1 decreases more than that of the conventional example.

[0106] In addition, it can be seen that over time, the tensile force of Example 2 decreases more than that of Example 1.

[0107] Finally, it can be seen that, over time, the specimens of Example 3 have decreased the most relative to Example 2.

[0108]

Test 2

[0109] In order to measure the sealing state between the titanium alloy and the polymer using the samples of the conventional embodiment and embodiments 1-3, a sealing test was conducted after 1000 hours of constant temperature and humidity. The results are shown in FIG. Fig.10 shown.

[0110] The specimen used in the conventional embodiment and Examples 1-3 is a Ti-2 grade titanium alloy as shown in FIG. 9( a), having a width of 12 mm, a length of 40 mm, and a thickness of 3 mm, which is injection molded and bonded to the center of the titanium specimen manufactured by the process of the conventional embodiment and Examples 1-3.

[0111] In order to measure the bonding strength, after 1000 hours of constant temperature and humidity, a sealing test as shown in Figure 9(b) was carried out. The results are as follows Fig.10 shown.

[0112] like Fig.10 As shown in the figure, it can be seen that the sealing performance of Example 1 is better than that of the sample of the traditional embodiment.

[0113] In addition, it can be seen that the test piece of Example 2 has better sealing performance than the test piece of Example 1.

[0114] Finally, it can be seen that, compared with the test piece of Example 2, the test piece of Example 3 has the most excellent sealing performance.

[0115] Fig.9A A photograph of the sample of the constant temperature and humidity experiment is shown.

[0116] Fig. 9B A photograph of the constant temperature and humidity experimental equipment is shown.

[0117] [Industrial Applicability]

[0118] The present invention is a method for manufacturing a polymer-titanium bonding structure, and it promotes weight reduction and cost reduction of components by improving bonding strength and sealing between polymer and titanium.

Claims

1. A method for treating a titanium surface for bonding with a polymer, comprising: (a) a first etching step, wherein the titanium surface is etched with an acidic solution; (b) a first surface treatment step, wherein the titanium surface is subjected to ultrasonic treatment; (c) a second etching step, wherein the titanium surface is etched again with an acidic solution; (d) a second surface treatment step, wherein the titanium surface is again subjected to ultrasonic treatment; (e) a first silane coupling treatment step, wherein the titanium surface is subjected to ultrasonic treatment; (f) a third surface treatment step, in which the titanium surface is again subjected to ultrasonic treatment; (g) A second silane coupling treatment step, wherein the titanium surface is subjected to anodization treatment.

2. The titanium surface treatment method according to claim 1, characterized in that: In the step (e), in a solution containing 10-50wt.% of an alkaline solution and 0.1-1wt.% of a first silane coupling agent, ultrasonic treatment is performed at 30-70°C with an output of 400W and a frequency of 24-100kHz for 10-300 seconds, wherein in the alkaline solution, 1-10% of caustic soda, 1-10% of sodium carbonate and 1-10% of ammonium nitrate are mixed in a ratio of 3:1:

1.

3. The titanium surface treatment method according to claim 1, characterized in that: The step (f) is carried out in an acidic solution containing a mixture of at least two or more of sulfuric acid with a concentration of 1-10%, phosphoric acid with a concentration of 1-10% and nitric acid with a concentration of 1-10% or in an alkaline solution containing a mixture of at least two or more of caustic soda with a concentration of 1-10%, sodium carbonate with a concentration of 1-10% and ammonium nitrate with a concentration of 1-10%, at 30-70°C with an ultrasonic treatment of 400W and a frequency of 24-100kHz for 10-300 seconds.

4. The titanium surface treatment method according to claim 2, characterized in that: Step (g) in a solution containing 10-50 wt.% of an electrolyte solution and 0.1-1 wt.% of a second silane coupling agent, using a rectifier at 30-70°C and at 0.1-10 A / dm 2 The process is carried out for 1-30 minutes with a current density of 1000 ms and a positive pulse duration of 500 ms, wherein in the electrolyte solution, NaOH, KOH, Ca(OH)2 and NaHCO3 are mixed in a ratio of 3:1:1:

1.

5. The titanium surface treatment method according to claim 4, characterized in that: The first silane coupling agent and the second silane coupling agent are (RO)3Si-(CH2)3-NH2, (RO)3Si-(CH2)2-Si(OC2H5)3, (RO)3Si-(CH2)3-SH, (RO)3Si-CH=CH2, (RO)3Si-(CH3)3-OOC(CH3)C=CH2, (RO)3Si-(CH3)3-O-CHCH2O and (RO)3Si-(CH2) 15 A mixture of at least two or more of CH3.

6. The titanium surface treatment method according to claim 5, characterized in that: The first silane coupling agent and the second silane coupling agent are a mixture of different types.