A method for ultra-low temperature crystallization copper plating on the surface of micron ceramic particles
By cooling Cu(NO3)2 in ethanol to crystallize on the surface of ceramic particles and reducing it to Cu in a high-efficiency CuO composite powder reduction device, the environmental pollution and high cost problems in the copper plating method on the surface of ceramic particles are solved, and the process is simple. , environmentally friendly, low-cost copper cladding effect.
Patent Information
- Application Number
- CN202310166941.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-02-27
AI Technical Summary
Existing copper plating methods on the surface of ceramic particles have problems of environmental pollution and high costs. In particular, the electroplating method produces waste water and waste gas. The electroless plating method requires precious metal activation treatment and the waste liquid treatment is complicated.
The ultra-low temperature crystallization copper plating method is used to form a saturated solution by dissolving Cu(NO3)2 and ceramic particles in ethanol, cooling the temperature to cause Cu(NO3)2 to crystallize and precipitate on the surface of the ceramic particles, and then heating and decomposing it in a high-efficiency CuO composite powder reduction device. H2 is reduced to Cu to form a copper cladding layer.
This method saves Cu(NO3)2 raw materials, reduces waste liquid pollution, has a simple process, low cost, and is environmentally friendly, suitable for industrial applications, and can effectively control the thickness of the copper cladding layer.
Smart Images

Figure BDA0004096197520000031 
Figure BDA0004096197520000033 
Figure BDA0004096197520000035
Abstract
Description
Technical Field
[0001] This invention discloses an ultra-low temperature crystallization copper plating method on the surface of micron-sized ceramic particles, belonging to the field of ceramic particle surface treatment. Background Technology
[0002] Ceramic particles possess properties such as high strength, high hardness, high temperature resistance, friction and wear resistance, and chemical corrosion resistance. By plating copper onto the surface of ceramic particles, the surface is metallized, enabling wide applications in composite materials, wear-resistant materials, high-temperature resistant materials, and anti-oxidation coatings. Currently, the main surface treatment methods for ceramic particles are electroplating and chemical plating. Electroplating forms a coating on the particle surface through electrode reactions, but the wastewater and exhaust gas generated can cause environmental pollution. Chemical plating produces alloy coatings with good uniformity, but it typically requires activation treatment with precious metals, resulting in wastewater discharge and drawbacks such as high cost and complex wastewater treatment processes. Summary of the Invention
[0003] The purpose of this invention is to provide a method for ultra-low temperature crystallization copper plating on the surface of micron-sized ceramic particles, specifically including the following steps:
[0004] (1) Add the pretreated ceramic particles and Cu(NO3)2 to ethanol and stir magnetically for 30 minutes to obtain a Cu(NO3)2 ethanol saturated mixed solution containing ceramic particles; wherein the mass of the pretreated ceramic particles: the mass of copper nitrate: the mass of ethanol is (15-20):(95-100):100.
[0005] (2) Place the mixed solution into a low temperature constant temperature test chamber and lower the temperature to an ultra-low temperature of -50℃ to -100℃. Then, perform magnetic stirring for 0.5-1h to reduce the solubility of Cu(NO3)2 in ultra-low temperature ethanol and crystallize it on the surface of ceramic particles. After filtering and separating the mixed solution at ultra-low temperature, place it in a room temperature environment to obtain ceramic particles with a Cu(NO3)2 film on the surface. After heating and decomposing them, ceramic particles with a CuO film on the surface are obtained.
[0006] Preferably, the process of reducing the ceramic particles coated with a CuO film according to the present invention is as follows: the ceramic particles coated with a CuO film are placed in the reduction tank of the high-efficiency CuO composite powder reduction device and heated to 400℃-500℃. H2 is introduced into the reduction tank through the inlet pipe at a flow rate of 4-7L / min. The power input device is started to rotate the reduction tank at a speed of 14-17r / min, so that the powder and H2 are in full contact. After efficient reduction for 1-2 hours, ceramic particles coated with a Cu film are obtained. The generated waste gas is discharged through a breathable mesh, a porous flange, and an exhaust pipe.
[0007] Preferably, the ceramic particles of the present invention are one of TiB2, SiC, Al2O3, SiO2, and BN with a particle size of 1-100 μm.
[0008] Preferably, the pretreatment of the ceramic particles of the present invention involves adding the ceramic particles to a 20% H2SO4 solution, stirring magnetically for 30 minutes, filtering, repeatedly washing with deionized water until neutral, and then placing them in a drying oven at 150°C for 1 hour to dry for later use.
[0009] Preferably, the heating decomposition of the present invention specifically involves heating ceramic particles coated with a Cu(NO3)2 film to 300℃-500℃ for 1-4 hours to decompose the Cu(NO3)2 on the surface of the ceramic particles into CuO, thereby obtaining ceramic particles coated with a CuO film.
[0010] Principle of this invention:
[0011] 1. Principle of Ultra-Low Temperature Crystallization Copper Plating
[0012] Ultra-low temperature crystallization copper plating is achieved by adding pretreated ceramic particles and Cu(NO3)2 to ethanol (melting point -114.1℃) at room temperature to obtain a saturated mixed solution of Cu(NO3)2 and ethanol containing ceramic particles. Figure 1 The curve showing the measured solubility of Cu(NO3)2 in ultra-low temperature ethanol as a function of temperature is derived from... Figure 1 It is known that the solubility of Cu(NO3)2 in ethanol at room temperature (20℃-30℃) and -100℃ is quite different. Therefore, Cu(NO3)2 is dissolved in ethanol at room temperature (20℃-30℃), and the preferred cooling range is -50℃ to -100℃.
[0013] Ethanol has a low melting point (-114.1℃), and Cu(NO3)2 exhibits high solubility in ultra-low temperature ethanol. This invention involves adding Cu(NO3)2 to room-temperature ethanol containing ceramic particles to form a saturated solution. The temperature is then lowered to an ultra-low temperature of -50℃ to -100℃, reducing the solubility of Cu(NO3)2 in ethanol and causing it to crystallize and precipitate on the surface of the ceramic particles. The ceramic particles coated with Cu(NO3)2 are then heated and decomposed, and placed into the high-efficiency CuO composite powder reduction device of this invention (attached). Figure 3 In this process, after heating, H2 is introduced and the powder is rotated to ensure full contact between the powder and the gas, thereby efficiently reducing CuO to Cu. Since ultra-low temperature crystallization uses a room-temperature Cu(NO3)2 / ethanol saturated solution to physically cool the ceramic particles, Cu(NO3)2 is coated onto the surface of the ceramic particles. This saves Cu(NO3)2 raw materials and reduces environmental pollution from waste liquid. It features a simple process, low cost, environmental friendliness, and high efficiency, making it suitable for industrial application.
[0014] 2. Principle of Copper Cladding Thickness Control
[0015] The ceramic particles and Cu(NO3)2 were added to ethanol in a ratio of ceramic particle mass: copper nitrate mass: ethanol mass = (15-20):(95-100):100. By adjusting the cooling temperature of the saturated Cu(NO3)2 ethanol solution containing ceramic particles, the solubility of Cu(NO3)2 in ultra-low temperature ethanol was reduced, thereby causing it to crystallize and precipitate on the surface of the ceramic particles. Figure 1 The solubility R of Cu(NO3)2 in ethanol can be calculated from the curve of Cu(NO3)2 solubility versus temperature and the fitting equation (1). T :
[0016]
[0017] (1) Where T is the temperature in °C; R is the temperature in °C. T —Solubility of Cu(NO3)2 in ethanol at T℃, g / 100g ethanol.
[0018] Based on the difference in solubility of Cu(NO3)2 in room temperature and ultra-low temperature ethanol in equation (1), the mass of Cu(NO3)2 precipitated on the surface of ceramic particles, M1, can be obtained:
[0019] M1 = R T1 -R T2 (2)
[0020] (2) In the formula, M1—Cu(NO3)2 precipitated on the surface of ceramic particles, g / 100g ethanol; R T1 —Solubility of Cu(NO3)2 in ethanol at room temperature, g / 100g ethanol; R T2 —Solubility of Cu(NO3)2 in ultra-low temperature ethanol, g / 100g ethanol.
[0021] Based on equation (2) and the ratio of the relative molecular masses of Cu(NO3)2 to CuO in the chemical formula for the thermal decomposition of Cu(NO3)2 into CuO, the mass M2 of Cu(NO3)2 decomposed into CuO by heating can be obtained:
[0022]
[0023]
[0024] M2 = 0.42(R) T1 -R T2 (3)
[0025] (3) In the formula, M1—Cu(NO3)2 precipitated on the surface of ceramic particles, g / 100g ethanol; M2—Cu(NO3)2 decomposed into CuO by heating, g / 100g ethanol; R T1 —Solubility of Cu(NO3)2 in ethanol at room temperature, g / 100g ethanol; R T2 —Solubility of Cu(NO3)2 in ultra-low temperature ethanol, g / 100g ethanol.
[0026] Based on equation (3) and the ratio of the relative molecular masses of CuO to Cu in the chemical formula for the reduction of CuO to Cu by heating in H2 atmosphere, the mass M3 of CuO to Cu by heating can be obtained:
[0027]
[0028]
[0029] M3 = 0.34(R) T1 -R T2 (4)
[0030] (4) In the formula, M2—Cu(NO3)2 decomposes into CuO by heating, g / 100g ethanol; M3—CuO is reduced to Cu by heating in H2 atmosphere, g / 100g ethanol; R T1 —Solubility of Cu(NO3)2 in ethanol at room temperature, g / 100g ethanol; R T2 —Solubility of Cu(NO3)2 in ultra-low temperature ethanol, g / 100g ethanol.
[0031] Based on the density formula, ceramic particle size, and mass, the formula for calculating the surface area of ceramic particles can be obtained:
[0032]
[0033] (5) In the formula, S—the surface area of ceramic particles, cm² 2 ρ1—Density of ceramic particles, g / cm³ 3 m—mass of ceramic particles, g / 100g ethanol; r—particle size of ceramic particles, μm.
[0034] Based on the ratio of ceramic particle mass: copper nitrate mass: ethanol mass = (15-20):(95-100):100 and combined with equations (1), (2), (3), (4) and (5), according to the molecular mass of the reactants, the thickness calculation formulas (6), (7), and (8) for Cu(NO3)2, CuO, and Cu can be derived.
[0035]
[0036]
[0037]
[0038] In equations (6)-(8), —Average thickness of Cu(NO3)2 coating, μm; δ CuO —Average thickness of CuO coating, μm; δ Cu —Average thickness of Cu coating, μm; S—Surface area of ceramic particles, cm² 2 M1—Mass of Cu(NO3)2 precipitated on the surface of ceramic particles, g / 100g ethanol; M2—Mass of Cu(NO3)2 decomposed into CuO upon heating, g / 100g ethanol; M3—Mass of CuO reduced to Cu upon heating in H2 atmosphere, g / 100g ethanol; ρ1—Density of ceramic particles, g / cm³ 3 The density of ρ2—Cu(NO3)2, ρ2=2.32g / cm³ 3 The density of ρ3—CuO, ρ3=6.31g / cm³ 3 ρ4—the density of Cu, ρ4 = 8.96 g / cm³ 3 m—mass of ceramic particles, g / 100g ethanol; r—particle size of ceramic particles, μm; R T1 —Solubility of Cu(NO3)2 in ethanol at room temperature, g / 100g ethanol; R T2 —Solubility of Cu(NO3)2 in ultra-low temperature ethanol, g / 100g ethanol.
[0039] 3. Selection of temperature and time for the thermal decomposition and reduction of Cu(NO3)2
[0040] At 170℃, Cu(NO3)2 is easily decomposed by heat, and the decomposition is complete at 250℃; if heated to above 600℃, some CuO will be converted into Cu2O. In order to completely decompose the Cu(NO3)2 coating on the surface of ceramic particles into CuO, the selected decomposition temperature is 300℃-500℃, and the decomposition time is 1-4h.
[0041] The Gibbs free energy change of CuO reduced to Cu by heating in H2 atmosphere ( Figure 2 It can be seen that the Gibbs free energy is negative in the temperature range of 25℃-850℃, therefore the reduction reaction can proceed spontaneously. However, at temperatures below 400℃, the reduction time is long and the efficiency is low. The high-efficiency CuO composite powder reduction device of this invention (attached) Figure 3 The reduction temperature is 400℃-500℃, and the reduction time is 1-2h.
[0042] The beneficial effects of this invention are:
[0043] The ultra-low temperature crystallization described in this invention involves physically cooling a saturated Cu(NO3)2 / ethanol solution at room temperature to coat the surface of ceramic particles with Cu(NO3)2. The Cu(NO3)2 on the ceramic particle surface is then heated and decomposed into CuO, which is then placed into the high-efficiency CuO composite powder reduction device of this invention (see attached diagram). Figure 3 In the process of heating, H2 is introduced and the powder is rotated to allow it to come into full contact with H2, thereby efficiently reducing CuO to Cu and achieving copper coating on the surface of ceramic particles. This invention can save Cu(NO3)2 raw materials and reduce environmental pollution caused by waste plating solution. It has the characteristics of simple process, low cost, environmental protection and high efficiency, and can be applied industrially. Attached Figure Description
[0044] Figure 1 The curve shows the solubility of Cu(NO3)2 in ultra-low temperature ethanol as a function of temperature.
[0045] Figure 2 This represents the change in Gibbs free energy of CuO reduced to Cu in a H2 atmosphere at 25℃-850℃.
[0046] Figure 3 Schematic diagram of a high-efficiency CuO composite powder reduction device.
[0047] Figure 3 In the middle: 1-Power input device; 2-Exhaust pipe; 3-Intake pipe; 4-Heating furnace; 5-Reduction device shell; 6-Sealing ring; 7-Perforated flange cover; 8-Ventilation mesh; 9-Reduction tank; 10-First bevel gear; 11-Bearing; 12-Sealed bearing; 13-Support frame; 14-Ceramic particles coated with CuO film; 15-Thermocouple; 16-Second bevel gear.
[0048] Figure 4 This is a flowchart of the ultra-low temperature crystallization copper plating process on the surface of ceramic particles. Detailed Implementation
[0049] The apparatus used in the embodiments of the present invention is as follows: Figure 3The device includes a power input device 1, an exhaust pipe 2, an intake pipe 3, a heating furnace 4, a reduction device housing 5, a sealing ring 6, a perforated flange cover 7, a vent mesh 8, a reduction tank 9, a first bevel gear 10, a bearing 11, a sealed bearing 12, a support frame 13, ceramic particles 14 coated with a CuO film 14, a thermocouple 15, and a second bevel gear 16. The output shaft of the power input device 1 passes through the heating furnace 4 and the reduction device housing 5 in sequence and connects to the first bevel gear 10. The second bevel gear 16 meshes with the first bevel gear 10. A reduction tank 9 has a [missing information - likely a component or structure]. The rotating shaft has an air inlet on the other side. The rotating shaft and the air inlet are fixed to the support frame 13 by bearing 11. The air inlet pipe 3 is connected to the air inlet, and a sealing ring 6 is provided at the connection. The rotating shaft is connected to the second bevel gear 16. The support frame 13 is placed at the bottom of the reduction device housing 5. The top of the reduction tank 9 is provided with a venting mesh 8 and a perforated flange cover 7. A sealing bearing 12 and a venting mesh 8 are provided at the air inlet. The top of the heating furnace 4 is provided with an exhaust pipe 2, and the bottom of the heating furnace 4 is provided with a thermocouple 15. A sealing ring is provided at the connection between the air inlet pipe 3 and the reduction device housing 5.
[0050] Example 1
[0051] A method for ultra-low temperature crystallization copper plating on the surface of micron-sized TiB2 powder, characterized by the following steps:
[0052] (1) Raw material pretreatment: Add commercially available TiB2 powder with a particle size of 1μm to a 20% H2SO4 solution and stir magnetically for 30 minutes. Then wash repeatedly with deionized water until neutral and place in a drying oven at 150℃ for 1 hour to dry for later use.
[0053] (2) Obtaining a mixed solution: Prepare materials according to the ratio of TiB2 powder mass: copper nitrate mass: ethanol mass = 20: 95: 100. Add TiB2 powder and Cu(NO3)2 to ethanol at room temperature (20℃) and stir magnetically for 20 minutes to obtain a saturated mixed solution of Cu(NO3)2 and ethanol containing TiB2 powder.
[0054] (3) Cu(NO3)2 coated TiB2 powder: The mixed solution obtained in step (2) was placed in a low temperature constant temperature test chamber and the temperature was lowered to -50℃. Then, it was magnetically stirred for 1 hour to reduce the solubility of Cu(NO3)2 in ethanol at ultra-low temperature and crystallize on the surface of TiB2 powder. The mixed solution was filtered at ultra-low temperature to separate the TiB2 powder and placed in a room temperature environment to obtain TiB2 powder with a Cu(NO3)2 film with a thickness of 0.46μm on the surface.
[0055] (4) CuO-coated TiB2 powder: The TiB2 powder coated with Cu(NO3)2 film obtained in step 3 is heated to 500℃ for 1 hour to decompose the Cu(NO3)2 on the surface of the TiB2 powder into CuO, and TiB2 powder with a 0.07μm thick CuO film on the surface is obtained.
[0056] (5) Cu-coated TiB2 powder: The TiB2 powder coated with CuO film obtained in step 4 is placed in the reduction tank 9 of the high-efficiency CuO composite powder reduction device and heated to 500°C. H2 is introduced into the reduction tank 9 through the inlet pipe 3 at a flow rate of 7L / min. The power input device 1 is started to rotate at a speed of 14r / min so that the powder and H2 are in full contact. After efficient reduction for 1h, TiB2 powder with a Cu film coated with a thickness of 0.04μm is obtained. The generated waste gas is discharged through the breathable mesh 8, the porous flange 7, and the exhaust pipe 2.
[0057] Example 2
[0058] A method for ultra-low temperature crystallization copper plating on the surface of micron-sized SiC powder, characterized by the following steps:
[0059] (1) Raw material pretreatment: Add commercially available SiC powder with a particle size of 30μm to a 20% H2SO4 solution and stir magnetically for 30 minutes. Then wash repeatedly with deionized water until neutral and place in a drying oven at 150℃ for 1 hour to dry for later use.
[0060] (2) Obtaining a mixed solution: Prepare materials according to the ratio of SiC powder mass: copper nitrate mass: ethanol mass = 18:97:100. Add SiC powder and Cu(NO3)2 to ethanol at room temperature (23℃) and stir magnetically for 20 minutes to obtain a saturated mixed solution of Cu(NO3)2 and ethanol containing SiC powder.
[0061] (3) Cu(NO3)2 coated SiC powder: The mixed solution obtained in step 2 was placed in a low temperature constant temperature test chamber and the temperature was lowered to -65℃. Then, it was magnetically stirred for 0.8h to reduce the solubility of Cu(NO3)2 in ethanol at ultra-low temperature and crystallize on the surface of SiC powder. The mixed solution was filtered at ultra-low temperature to separate the SiC powder and placed in a room temperature environment to obtain SiC powder with a 16.6μm thick Cu(NO3)2 film on the surface.
[0062] (4) CuO-coated SiC powder: The SiC powder coated with Cu(NO3)2 film obtained in step 3 is heated to 435℃ for 2 hours to decompose and transform Cu(NO3)2 on the surface of SiC powder into CuO, so as to obtain SiC powder with a 2.6μm thick CuO film on the surface.
[0063] (5) Cu-coated SiC powder: The SiC powder coated with a CuO film obtained in step 4 is placed into a high-efficiency CuO composite powder reduction device (attached). Figure 3 The powder is heated to 475°C in the reduction tank 9. H2 is introduced into the reduction tank 9 through the inlet pipe 3 at a flow rate of 6L / min. The power input device 1 is started to rotate at a speed of 15r / min, so that the powder and H2 are in full contact. After efficient reduction for 1.3h, SiC powder with a 1.4μm thick Cu film on the surface is obtained. The generated waste gas is discharged through the breathable mesh 8, the porous flange 7, and the exhaust pipe 2.
[0064] Example 3
[0065] A method for ultra-low temperature crystallization copper plating on the surface of micron-sized SiO2 powder, characterized by the following steps:
[0066] (1) Raw material pretreatment: Add commercially available SiO2 powder with a particle size of 60μm to a 20% H2SO4 solution and stir magnetically for 30 minutes. Then wash repeatedly with deionized water until neutral and place in a drying oven at 150℃ for 1 hour to dry for later use.
[0067] (2) Obtaining a mixed solution: Prepare materials according to the ratio of SiO2 powder mass: copper nitrate mass: ethanol mass = 17:98:100. Add SiO2 powder and Cu(NO3)2 to ethanol at room temperature (27℃) and stir magnetically for 20 minutes to obtain a saturated mixed solution of Cu(NO3)2 and ethanol containing SiO2 powder.
[0068] (3) Cu(NO3)2 coated SiO2 powder: The mixed solution obtained in step 2 was placed in a low temperature constant temperature test chamber and the temperature was lowered to -85℃. Then, it was magnetically stirred for 0.7h to reduce the solubility of Cu(NO3)2 in ultra-low temperature ethanol and crystallize and precipitate on the surface of SiO2 powder, so as to obtain SiO2 powder with a Cu(NO3)2 film coated on the surface.
[0069] (4) CuO-coated SiO2 powder: The SiO2 powder coated with Cu(NO3)2 film obtained in step 3 is heated to 375°C and decomposed for 3 hours, so that Cu(NO3)2 on the surface of SiO2 powder decomposes into CuO, and SiO2 powder with a 5.0μm thick CuO film is obtained.
[0070] (5) Cu-coated SiO2 powder: The SiO2 powder coated with a CuO film obtained in step 4 is placed into a high-efficiency CuO composite powder reduction device (attached). Figure 3The powder is heated to 435°C in the reduction tank 9. H2 is introduced into the reduction tank 9 through the inlet pipe 3 at a flow rate of 5L / min. The power input device 1 is started to rotate at a speed of 16r / min, so that the powder and H2 are in full contact. After efficient reduction for 1.7h, SiO2 powder with a 2.8μm thick Cu film on the surface is obtained. The generated waste gas is discharged through the breathable mesh 8, the porous flange 7, and the exhaust pipe 2.
[0071] Example 4
[0072] A method for ultra-low temperature crystallization copper plating on the surface of micron-sized BN powder, characterized by the following steps:
[0073] (1) Raw material pretreatment: Add commercially available BN powder with a particle size of 100μm to a 20% H2SO4 solution and stir magnetically for 30 minutes. Then wash repeatedly with deionized water until neutral and place in a drying oven at 150℃ for 1 hour to dry for later use.
[0074] (2) Obtaining a mixed solution: Prepare materials according to the ratio of BN powder mass: copper nitrate mass: ethanol mass = 15:100:100. Add BN powder and Cu(NO3)2 to ethanol at room temperature (30℃) and stir magnetically for 20 minutes to obtain a saturated mixed solution of Cu(NO3)2 and ethanol containing BN powder.
[0075] (3) Cu(NO3)2 coating BN powder: The mixed solution obtained in step 2 was placed in a low temperature constant temperature test chamber and the temperature was lowered to -100℃. Then, it was magnetically stirred for 0.5h to reduce the solubility of Cu(NO3)2 in ethanol at ultra-low temperature and crystallize on the surface of BN powder. The mixed solution was filtered at ultra-low temperature to separate the BN powder and placed in a room temperature environment to obtain BN powder with a Cu(NO3)2 film with a thickness of 77.6μm.
[0076] (4) CuO-coated BN powder: The BN powder coated with Cu(NO3)2 film obtained in step 3 is heated to 300℃ for 4 hours to decompose the Cu(NO3)2 on the surface of the BN powder into CuO, and BN powder with a 12.0μm thick CuO film on the surface is obtained.
[0077] (5) Cu-coated BN powder: The BN powder coated with a CuO film obtained in step 4 is placed into a high-efficiency CuO composite powder reduction device (attached). Figure 3The powder is heated to 400°C in the reduction tank 9. H2 is introduced into the reduction tank 9 through the inlet pipe 3 at a flow rate of 4L / min. The power input device 1 is started to rotate at a speed of 17r / min, so that the powder and H2 are in full contact. After efficient reduction for 2 hours, BN powder with a 6.6μm thick Cu film on the surface is obtained. The generated waste gas is discharged through the breathable mesh 8, the porous flange 7, and the exhaust pipe 2.
Claims
1. A method for ultra-low temperature crystallization copper plating on the surface of micron ceramic particles, characterized in that: The specific steps include: (1) adding the pretreated ceramic particles and Cu(NO3)2 into ethanol and magnetically stirring for 30 minutes to obtain a saturated mixed solution of Cu(NO3)2 ethanol containing ceramic particles; wherein the mass of the pretreated ceramic particles: the mass of copper nitrate: the mass of ethanol is (15-20): (95-100): 100; (2) placing the mixed solution in a low-temperature constant temperature experimental box, lowering the temperature to an ultra-low temperature of -50°C to -100°C, and then magnetically stirring for 0.5-1h to reduce the solubility of Cu(NO3)2 in ultra-low temperature ethanol and crystallize on the surface of ceramic particles; filtering and separating the mixed solution at ultra-low temperature, and placing it in a room temperature environment to obtain ceramic particles with a Cu(NO3)2 film on the surface; heating and decomposing the mixed solution to obtain ceramic particles with a CuO film on the surface; The reduction process of the ceramic particles coated with CuO film on the surface is as follows: the ceramic particles coated with CuO film on the surface are placed in a reduction tank of a high-efficiency CuO composite powder reduction device and heated to 400°C-500°C, H2 is introduced into the reduction tank from an intake pipe at a flow rate of 4-7L / min, a power input device is started, and the reduction tank is rotated at a speed of 14-17r / min to make the powder fully contact with H2, and ceramic particles coated with Cu film on the surface are obtained after high-efficiency reduction for 1-2h, and the generated exhaust gas is discharged through a breathable net, a porous flange, and an exhaust pipe; The ceramic particles are one of TiB2, SiC, Al2O3, SiO2 and BN with a particle size of 1-100 μm.
2. The method for ultra-low temperature crystallization copper plating on the surface of micron ceramic particles according to claim 1, characterized in that: The pretreatment of ceramic particles is to add the ceramic particles to a 20% H2SO4 solution, stir magnetically for 30 minutes, filter, wash repeatedly with deionized water until neutral, place in a drying oven at 150°C for 1 hour, and dry for use.
3. The method for ultra-low temperature crystallization copper plating on the surface of micron ceramic particles according to claim 1, characterized in that: The thermal decomposition is specifically as follows: the ceramic particles with the surface coated with Cu(NO3)2 film are heated to 300℃-500℃ and decomposed for 1-4h, so that the Cu(NO3)2 on the surface of the ceramic particles is decomposed and converted into CuO, thereby obtaining ceramic particles with the surface coated with CuO film.