A broadband high permeability MnZn ferrite and its preparation method

By optimizing the ratio and process of MnZn ferrite, a material with higher magnetic permeability and temperature stability in a wide frequency range is prepared, which solves the problem of insufficient performance of existing materials and is suitable for electronics in high-frequency and high-temperature difference environments. equipment.

CN116143510BActive Publication Date: 2024-10-22CHANGSHU HAOBO ELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111386787.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-22
Publication Date
2024-10-22
Estimated Expiration
2041-11-22

AI Technical Summary

Technical Problem

The existing high magnetic permeability MnZn ferrite materials have insufficient performance in a wide frequency range, and the manufacturing process is complex, resulting in poor performance and unable to meet the needs of electrical equipment and telecommunications facilities for higher magnetic permeability and wider frequencies.

Method used

Using the ratio of main components Fe2O3, ZnO and MnO, adding auxiliary components Bi2O3, MoO3, SiO2, CaO, V2O5, Nb2O5 and Co2O3, and using PVA binder, 1-methylpentanol dispersant and silicone defoaming Agent, broadband high permeability MnZn ferrite is prepared through wet ball milling, pre-sintering, secondary grinding, granulation, pressing and sintering.

Benefits of technology

It provides higher magnetic permeability and good temperature stability in an ultra-wide temperature range. It is suitable for electronic products with high temperature difference environments and high stability requirements, such as energy-saving lamps and communication equipment, and has low loss and high saturation magnetic induction intensity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a broadband high-permeability MnZn ferrite and a preparation method thereof, and relates to the technical field of MnZn ferrite preparation. The broadband high-permeability MnZn ferrite and preparation method thereof, the broadband high-permeability MnZn ferrite comprises a main component, an auxiliary component, a binder, a dispersant and a defoaming agent, the main component comprises 52.0-53.0 mol% of Fe2O3, 20.0-22.0 mol% of ZnO and 25.0-28.0 mol% of MnO, the auxiliary component comprises 200-500 ppm of Bi2O3, 100-500 ppm of MoO3, 50-150 ppm of SiO2, 100-200 ppm of CaO, 100-200 ppm of V2O5, 100-200 ppm of Nb2O5, 200-500 ppm of TiO2, 100-400 ppm of Co2O3, and the grain size of the auxiliary component is less than 20 μm. The present invention provides a broadband high-permeability MnZn ferrite and a preparation method thereof. The broadband high-permeability MnZn ferrite material of the present invention has higher magnetic permeability (the magnetic permeability reaches above 15000), better frequency characteristics, lower specific loss, and its technical indicators are better than many currently available materials and its performance is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of MnZn ferrite preparation, in particular to a broadband high-permeability MnZn ferrite and a preparation method thereof. Background Art

[0002] High permeability MnZn ferrite materials are developed to meet the needs of high inductance and small and light electronic communications and new electronic lighting equipment. They are widely used, especially in today's communications field. Digital network communications and optical fiber communications technology and equipment are developing at a rapid pace. There is an urgent need for electronic devices such as filters, broadband transformers and pulse transformers made of high permeability MnZn ferrite cores.

[0003] With the development of society and the improvement of living standards, people have higher and higher requirements for electrical equipment and telecommunication facilities, stricter product requirements, wider application scope requirements, and higher requirements for magnetic materials. Not only higher magnetic permeability is required, but also wider application frequency is required. For example, materials with a magnetic permeability of 10,000-12,000 are required to have a starting magnetic permeability μi value that remains flat at around 100kHz. In order to make the device have better performance in the same volume or a smaller volume with the same performance, and to meet the market demand for miniaturization and high efficiency of products, it is urgent to develop broadband high permeability materials with higher magnetic permeability.

[0004] The existing patent (publication number: CN102108022A) discloses a manganese-zinc soft magnetic ferrite material with a wide temperature range and a low temperature coefficient and a preparation method thereof. The material consists of a main component and an additive, wherein the composition formula of the main component is: 68-72wt% Fe2O3, 11-15wt% ZnO, and the balance is Mn3O4; the composition formula of the additive is: 0.015-0.05wt% CaCO3, 0.1-0.4wt% Co2O3, 0.001-0.005wt% SiO2, 0.02-0.07wt% V2O5, 0.02-0.07wt% Nb2O5, 0.05-0.1wt% TiO2 and 0.02-0.07wt% SnO2, and the mass percentage of each component in the additive formula is calculated relative to the total mass of the main component. The manganese-zinc soft ferrite material of the present invention has not only low loss and high Bs, but also a low temperature coefficient in the range of -40 to +100°C, and can be applied to electronic products such as communication transformers and energy-saving lamps used in environments with large temperature differences. However, the initial permeability range is not described, and the formula has 7 additives, and 0.25wt% of analytically pure Fe2O3 of the total mass of the main component must be added during sand grinding, so the manufacturing process is relatively complicated and the performance of the prepared product is also relatively poor. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides a broadband high permeability MnZn ferrite and a preparation method thereof, which solves the problem that people have increasingly higher requirements for electrical equipment and telecommunication facilities, increasingly stringent product requirements, increasingly wider application range requirements, and increasingly higher requirements for magnetic materials, requiring not only higher permeability but also wider application frequency.

[0007] (II) Technical solution

[0008] To achieve the above objectives, the present invention is implemented through the following technical scheme: a broadband high permeability MnZn ferrite, the broadband high permeability MnZn ferrite includes a main component, an auxiliary component, a binder, a dispersant and a defoaming agent, the main component includes 52.0-53.0mol% Fe2O3, 20.0-22.0mol% ZnO and 25.0-28.0mol%, the auxiliary component includes 200-500ppm Bi2O3, 100-500ppm MoO3, 50-150ppm SiO2, 100-200ppm CaO, 100-200ppm V2O5, 100-200ppm Nb2O5, 200-500ppm TiO2, 100-400ppm Co2O3, and the grain size of the auxiliary component is less than 20μm.

[0009] Preferably, the weight composition of the auxiliary components, in proportion to the total weight of the components, is: Bi2O3 0.03-0.08wt%, MoO3 0.02-0.05wt%, SiO2 0.006-0.012wt%, CaO 0.01-0.045wt%, V2O5 0.02-0.06wt%, Nb2O5 0.03-0.07wt%, TiO2 0.01-0.26wt%, Co2O3 0.02-0.06wt%.

[0010] Preferably, the binder is a PVA binder, and its content is 0.4 wt % calculated based on the total mass.

[0011] Preferably, the dispersant is 1-methylpentanol dispersant, and its content is 0.4 wt % calculated based on the total mass.

[0012] Preferably, the defoaming agent is a silicone defoaming agent, and its content is 0.3 wt % calculated based on the total mass.

[0013] Preferably, a method for preparing a broadband high permeability MnZn ferrite specifically comprises the following steps:

[0014] S1. Weighing the main components

[0015] Weigh the main components according to Fe2O3 52.0-53.0mol%, ZnO 20.0-22.0mol% and MnO 25.0-28.0mol%, and then mix them;

[0016] S2. Preliminary grinding

[0017] After mixing the weighed main components, put them into a ball mill for wet ball milling and grind for 20 to 40 minutes to make the main components fully mixed and uniform to obtain powder;

[0018] S3. Pre-sintering

[0019] The powder obtained in step S2 is dried, and then heated to 800°C-900°C at a heating rate of 200-250°C / h, pre-fired for 1-3 hours, and naturally cooled out of the furnace to obtain a pre-fired material;

[0020] S4. Secondary grinding

[0021] The pre-sintered material obtained in step S3 is wet-ground twice, and then the auxiliary components are added in sequence: 200-500 ppm Bi2O3, 100-500 ppm MoO3, 50-150 ppm SiO2, 100-200 ppm CaO, 100-200 ppm V2O5, 100-200 ppm Nb2O5, 200-500 ppm TiO2, and 100-400 ppm Co2O3, and the wet grinding is repeated for 30 min to 120 min using a ball mill to obtain a slurry;

[0022] S5. Granulation

[0023] Adding 0.4 wt % of a PVA binder, 0.4 wt % of a dispersant and 0.3 wt % of a defoamer calculated by total mass into the slurry in step S4 for spray granulation;

[0024] S6. Pressing

[0025] The granulated powder is pressed into a blank product, and the density of the blank is controlled at 2.60-2.85g / cm;

[0026] S7. Sintering

[0027] The formed blank product is sintered in an atmosphere bell furnace, the sintering temperature is controlled at 1350°C-1450°C, the insulation time is 6-12 hours, and then naturally cooled out of the furnace to obtain a broadband high permeability MnZn ferrite material.

[0028] Preferably, the particle size of the slurry after the secondary wet grinding in step S4 is less than 1.5 μm.

[0029] Preferably, in step S7, the blank product is sintered, kept warm, and then cooled to 180° C. before being taken out of the furnace.

[0030] (III) Beneficial effects

[0031] The present invention provides a broadband high permeability MnZn ferrite and a preparation method thereof. It has the following beneficial effects:

[0032] 1. The broadband high permeability MnZn ferrite and the preparation method thereof provided by the present invention have higher permeability and good temperature stability in an ultra-wide temperature range, and have an initial permeability greater than 3800 and less than 5000 at -60°C to 120°C, as well as a Curie temperature greater than 170°C and a saturation magnetic induction intensity greater than 480mT at room temperature. The ferrite can be used in an environment with a larger temperature difference, or in an environment with higher requirements for product stability, thereby better meeting market demand.

[0033] 2. The broadband high permeability MnZn ferrite and its preparation method provided by the present invention have low loss, high saturation magnetic flux density, and wide temperature and low temperature coefficient characteristics, namely: the specific loss coefficient (tanδ / -6μi) under the conditions of 25°C, 10KHz, and 0.25mT reaches 2 to 4×10; the saturation magnetic flux density (Bs) under the conditions of 25°C and 1194A / m reaches 475 to 495mT; under the conditions of 10KHz and 0.25mT, the specific temperature coefficient (αμ) in the range of -40°C to +100°C is 0.1 to -60.5×10 / °C; it can be widely used in ballasts of energy-saving lamps, filters of communication equipment, broadband pulse transformers, etc., and has a wider range of applications.

[0034] 3. The broadband high permeability MnZn ferrite and its preparation method provided by the present invention. The broadband high permeability MnZn ferrite material of the present invention has higher magnetic permeability (magnetic permeability reaches more than 15000), better frequency characteristics, lower specific loss, and its technical indicators are better than many existing materials, and its performance is better. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0036] An embodiment of the present invention provides a broadband high permeability MnZn ferrite, which includes a main component, an auxiliary component, a binder, a dispersant and a defoaming agent, wherein the main component includes 52.0 mol% of Fe2O3, 0.0 mol% of ZnO2 and 25.0 mol% of MnO, the auxiliary component includes 200-500 ppm of Bi2O3, 100-500 ppm of MoO3, 50-150 ppm of SiO2, 100-200 ppm of CaO, 100-200 ppm of V2O5, 100-200 ppm of Nb2O5, 200-500 ppm of TiO2, and 100-400 ppm of Co2O3, and the grain size of the auxiliary component is less than 20 μm.

[0037] The weight composition of the auxiliary components in proportion to the total weight of the components is: Bi2O3 0.03wt%, MoO3 0.02wt%, SiO2 0.006wt%, CaO 0.01wt%, V2O5 0.02wt%, Nb2O5 0.03wt%, TiO2 0.01wt%, Co2O3 0.02wt%

[0038] A method for preparing a broadband high permeability MnZn ferrite specifically comprises the following steps:

[0039] S1. Weighing the main components

[0040] The main components were weighed according to 52.0 mol% of Fe2O3, 20.0 mol% of ZnO and 25.0 mol% of MnO, and then mixed;

[0041] S2. Preliminary grinding

[0042] After mixing the weighed main ingredients, put them into a ball mill for wet ball milling and grind for 30 minutes to make the main ingredients fully mixed and uniform to obtain powder;

[0043] S3. Pre-sintering

[0044] The powder obtained in step S2 is dried, then heated to 800°C at a heating rate of 200°C / h, pre-fired for 2 hours, and naturally cooled and taken out of the furnace to obtain a pre-fired material;

[0045] S4. Secondary grinding

[0046] The pre-sintered material obtained in step S3 is wet-ground twice, and then the auxiliary components are added in sequence: 200-500 ppm Bi2O3, 100-500 ppm MoO3, 50-150 ppm SiO2, 100-200 ppm CaO, 100-200 ppm V2O5, 100-200 ppm Nb2O5, 200-500 ppm TiO2, and 100-400 ppm Co2O3, and the wet grinding is repeated for 60 min using a ball mill to obtain a slurry;

[0047] S5. Granulation

[0048] Adding 0.4 wt % of a PVA binder, 0.4 wt % of a dispersant and 0.3 wt % of a defoamer calculated by total mass into the slurry in step S4 for spray granulation;

[0049] S6. Pressing

[0050] The granulated powder is pressed into a blank product, and the density of the blank is controlled at 2.60g / cm;

[0051] S7. Sintering

[0052] The formed blank product is sintered in an atmosphere bell furnace with the sintering temperature controlled at 1350°C for 8 hours, and then naturally cooled out of the furnace to obtain a broadband and high permeability MnZn ferrite material. Example 2

[0053] An embodiment of the present invention provides a broadband high permeability MnZn ferrite, which includes a main component, an auxiliary component, a binder, a dispersant and a defoaming agent, wherein the main component includes 52.5 mol% of Fe2O3, 1.0 mol% of ZnO2 and 26.0 mol% of MnO; the auxiliary components include 200-500 ppm of Bi2O3, 100-500 ppm of MoO3, 50-150 ppm of SiO2, 100-200 ppm of CaO, 100-200 ppm of V2O5, 100-200 ppm of Nb2O5, 200-500 ppm of TiO2, and 100-400 ppm of Co2O3, and the grain size of the auxiliary components is less than 20 μm.

[0054] The weight composition of the auxiliary components in proportion to the total weight of the components is: Bi2O3 0.05wt%, MoO3 0.04wt%, SiO2 0.009wt%, CaO 0.03wt%, V2O5 0.04wt%, Nb2O5 0.05wt%, TiO2 0.018wt%, Co2O3 0.04wt%

[0055] A method for preparing a broadband high permeability MnZn ferrite specifically comprises the following steps:

[0056] S1. Weighing the main components

[0057] The main components were weighed according to 52.5 mol% of Fe2O3, 21.0 mol% of ZnO and 26.0 mol% of MnO, and then mixed;

[0058] S2. Preliminary grinding

[0059] After mixing the weighed main ingredients, put them into a ball mill for wet ball milling and grind for 35 minutes to make the main ingredients fully mixed and uniform to obtain powder;

[0060] S3. Pre-sintering

[0061] The powder obtained in step S2 is dried, then heated to 850°C at a heating rate of 225°C / h, pre-fired for 2.5 hours, and naturally cooled to obtain a pre-fired material;

[0062] S4. Secondary grinding

[0063] The pre-sintered material obtained in step S3 is wet-ground twice, and then the auxiliary components are added in sequence: 200-500 ppm Bi2O3, 100-500 ppm MoO3, 50-150 ppm SiO2, 100-200 ppm CaO, 100-200 ppm V2O5, 100-200 ppm Nb2O5, 200-500 ppm TiO2, and 100-400 ppm Co2O3, and the wet grinding is repeated for 90 min using a ball mill to obtain a slurry;

[0064] S5. Granulation

[0065] Adding 0.4 wt % of a PVA binder, 0.4 wt % of a dispersant and 0.3 wt % of a defoamer calculated by total mass into the slurry in step S4 for spray granulation;

[0066] S6. Pressing

[0067] The granulated powder is pressed into a blank product, and the density of the blank is controlled at 2.75g / cm;

[0068] S7. Sintering

[0069] The formed blank product is sintered in an atmosphere bell furnace with the sintering temperature controlled at 1400°C for 10 hours, and then naturally cooled out of the furnace to obtain a broadband and high permeability MnZn ferrite material. Example 3

[0070] An embodiment of the present invention provides a broadband high permeability MnZn ferrite, which includes a main component, an auxiliary component, a binder, a dispersant and a defoaming agent, wherein the main component includes 53.0 mol% of Fe2O3, 2.0 mol% of ZnO2 and 28.0 mol% of MnO; the auxiliary components include 200-500 ppm of Bi2O3, 100-500 ppm of MoO3, 50-150 ppm of SiO2, 100-200 ppm of CaO, 100-200 ppm of V2O5, 100-200 ppm of Nb2O5, 200-500 ppm of TiO2, and 100-400 ppm of Co2O3, and the grain size of the auxiliary components is less than 20 μm.

[0071] The weight composition of the auxiliary components in proportion to the total weight of the components is: Bi2O3 0.08wt%, MoO3 0.05wt%, SiO2 0.012wt%, CaO 0.045wt%, V2O5 0.06wt%, Nb2O5 0.07wt%, TiO2 0.26wt%, Co2O3 0.06wt%

[0072] A method for preparing a broadband high permeability MnZn ferrite specifically comprises the following steps:

[0073] S1. Weighing the main components

[0074] The main components were weighed according to 53.0 mol% of Fe2O3, 22.0 mol% of ZnO and 28.0 mol% of MnO, and then mixed;

[0075] S2. Preliminary grinding

[0076] After mixing the weighed main ingredients, put them into a ball mill for wet ball milling and grind for 40 minutes to make the main ingredients fully mixed and uniform to obtain powder;

[0077] S3. Pre-sintering

[0078] The powder obtained in step S2 is dried, then heated to 900°C at a heating rate of 250°C / h, pre-fired for 3 hours, and naturally cooled and taken out of the furnace to obtain a pre-fired material;

[0079] S4. Secondary grinding

[0080] The pre-sintered material obtained in step S3 is wet-ground twice, and then the auxiliary components are added in sequence: 200-500 ppm Bi2O3, 100-500 ppm MoO3, 50-150 ppm SiO2, 100-200 ppm CaO, 100-200 ppm V2O5, 100-200 ppm Nb2O5, 200-500 ppm TiO2, and 100-400 ppm Co2O3, and the wet grinding is repeated for 120 min using a ball mill to obtain a slurry;

[0081] S5. Granulation

[0082] Adding 0.4 wt % of a PVA binder, 0.4 wt % of a dispersant and 0.3 wt % of a defoamer calculated by total mass into the slurry in step S4 for spray granulation;

[0083] S6. Pressing

[0084] The granulated powder is pressed into a blank product, and the density of the blank is controlled at 2.85g / cm;

[0085] S7. Sintering

[0086] The formed blank product is sintered in an atmosphere bell furnace with the sintering temperature controlled at 1450°C for 12 hours, and then naturally cooled out of the furnace to obtain a broadband and high permeability MnZn ferrite material.

[0087] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A broadband high permeability MnZn ferrite, characterized in that: The broadband high permeability MnZn ferrite comprises a main component, an auxiliary component, a binder, a dispersant and a defoaming agent, wherein the main component comprises 52.0-53.0 mol% of Fe2O3, 0.0-22.0 mol% of ZnO2 and 5.0-28.0 mol% of MnO2, and the auxiliary component comprises 200-500 ppm of Bi2O3, 100-500 ppm of MoO3, 50-150 ppm of SiO2, 100-200 ppm of CaO, 100-200 ppm of V2O5, 100- 200ppm Nb2O5, 200-500ppm TiO2, 100-400ppm Co2O3, the grain size of the auxiliary components is less than 20μm.

2. A broadband high permeability MnZn ferrite according to claim 1, characterized in that: The weight composition of the auxiliary components, in proportion to the total weight of the components, is: Bi2O3 0.03-0.08wt%, MoO3 0.02-0.05wt%, SiO2 0.006-0.012wt%, CaO 0.01-0.045wt%, V2O5 0.02-0.06wt%, Nb2O5 0.03-0.07wt%, TiO2 0.01-0.26wt%, Co2O3 0.02-0.06wt%.

3. A broadband high permeability MnZn ferrite according to claim 1, characterized in that: The binder is a PVA binder, and its content is 0.4 wt % calculated based on the total mass.

4. The broadband high permeability MnZn ferrite according to claim 1, characterized in that: The dispersant is 1-methylpentanol dispersant, and its content is 0.4 wt % calculated based on the total mass.

5. The broadband high permeability MnZn ferrite according to claim 1, characterized in that: The defoamer is a silicone defoamer, and the content thereof is 0.3 wt % calculated based on the total mass.

6. A method for preparing broadband high permeability MnZn ferrite, characterized in that: The specific steps include: S1. Weighing the main components Weigh the main components according to Fe2O3 52.0-53.0mol%, ZnO2 0.0-22.0mol% and MnO2 5.0-28.0mol%, and then mix them; S2. Preliminary grinding After mixing the weighed main components, put them into a ball mill for wet ball milling and grind for 20 to 40 minutes to ensure that the main components are fully mixed and uniformly obtained into powder; S3. Pre-sintering The powder obtained in step S2 is dried, and then heated to 800°C-900°C at a heating rate of 200-250°C / h, pre-fired for 1-3 hours, and naturally cooled out of the furnace to obtain a pre-fired material; S4. Secondary grinding The pre-sintered material obtained in step S3 is wet-ground twice, and then the auxiliary components are added in sequence: 200-500 ppm Bi2O3, 100-500 ppm MoO3, 50-150 ppm SiO2, 100-200 ppm CaO, 100-200 ppm V2O5, 100-200 ppm Nb2O5, 200-500 ppm TiO2, and 100-400 ppm Co2O3, and the wet grinding is repeated for 30 min to 120 min using a ball mill to obtain a slurry; S5. Granulation Adding 0.4 wt % of a PVA binder, 0.4 wt % of a dispersant and 0.3 wt % of a defoamer calculated by total mass into the slurry in step S4 for spray granulation; S6. Pressing The granulated powder is pressed into a blank product, and the density of the blank is controlled at 2.60-2.85g / cm; S7. Sintering The formed blank product is sintered in an atmosphere bell furnace, the sintering temperature is controlled at 1350°C-1450°C, the insulation time is 6-12 hours, and then naturally cooled out of the furnace to obtain a broadband high permeability MnZn ferrite material.

7. The method for preparing a broadband high permeability MnZn ferrite according to claim 6, characterized in that: The particle size of the slurry after the secondary wet grinding in step S4 is less than 1.5 μm.

8. The method for preparing a broadband high permeability MnZn ferrite according to claim 6, characterized in that: In the step S7, the rough product is sintered, kept warm, and then cooled to 180° C. for removal from the furnace.