A method for vacuum synthesis of indium phosphide polycrystal
The vacuum synthesis method is used to process indium blocks and red phosphorus under a briquetting machine, which solves the problems of long synthesis time and low safety in the existing technology, achieves fast and high-purity polycrystalline synthesis of indium phosphide, and reduces costs and Energy consumption is reduced, and the process flow is simplified.
Patent Information
- Application Number
- CN202310179114.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-28
AI Technical Summary
The existing technology has the problems of long synthesis time, easy explosion, low safety, high cost when synthesizing indium phosphide polycrystalline, and it is difficult to control the pressure balance and purity.
Using the vacuum synthesis method, indium blocks and red phosphorus are mixed according to the designed mass ratio and pressed into small pieces under a briquetting machine. Vacuum heat treatment is performed to reduce the reaction temperature and gas phase pressure, avoid "tube explosion", simplify the process and reduce costs. .
Fast, safe and high-purity polycrystalline synthesis of indium phosphide has been achieved, reducing costs and energy consumption, simplifying the process and improving product quality.
Smart Images

Figure HDA0004102017700000011 
Figure HDA0004102017700000012 
Figure HDA0004102017700000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of compound semiconductor material preparation, and in particular relates to a method for vacuum synthesizing indium phosphide polycrystal. Background Art
[0002] Indium phosphide is an important III-V semiconductor material with a zinc blende structure, a brittle texture, and a silver-gray luster. As a second-generation semiconductor, indium phosphide has more outstanding electrical properties. Its direct transition band gap is 1.35eV, corresponding to the band with the smallest transmission loss in optical communications. It has better thermal conductivity and heat dissipation performance, and indium phosphide has more advantages in device manufacturing. In addition, the high current peak-to-valley ratio of InP devices determines the high conversion efficiency of the device; and InP devices have better noise characteristics; InP-based materials have high operating temperatures and strong radiation resistance, and have high conversion efficiency as solar cell materials. The realization of the above-mentioned high-end InP-based microelectronics and optoelectronic devices needs to be based on indium phosphide polycrystals with high technical standards.
[0003] Indium phosphide polycrystals are directly formed by the combination of high-purity indium and high-purity red phosphorus. When InP is at a temperature near the melting point of 1335±7K, its dissociation pressure is 2.75MPa. Under this condition, the phosphorus vapor pressure has exceeded 10MPa, which is much greater than the dissociation pressure of indium phosphide. Therefore, it is very difficult to synthesize indium phosphide single crystals directly from phosphorus and indium in a single crystal furnace. Generally, high-purity indium and high-purity phosphorus are synthesized into polycrystals and then indium phosphide polycrystals are used to grow indium phosphide single crystals. At present, there are mainly the following methods for synthesizing InP polycrystals: horizontal gradient solidification method (HGF), horizontal Bridgman method (HB), solute diffusion method (SSD), direct synthesis method, etc.; among them, the SSD method mainly uses diffusion, and its synthesis temperature is low, so the purity of the synthesis is high, but the amount of synthesis is small and the speed is slow, resulting in high cost, and it is basically no longer used; the synthesis principle of the HB method and the HGF method is similar to the SSD method, the synthesis amount is larger than the SSD method, and the speed is also much improved. It is the main method for producing indium phosphide polycrystals in industry, but the pressure balance is not easy to control, it is easy to "explode the tube", and the synthesis time is long , it is inevitable that more Si will diffuse into the polycrystal, reducing the purity of the polycrystal; the in-situ phosphorus injection method is an in-situ direct synthesis technology, which mainly uses the pressure difference between the inside and outside of the phosphorus bubble to inject phosphorus vapor into the indium melt. This method has a fast synthesis rate and can achieve one-step synthesis and growth, thereby improving the purity of the InP crystal. However, this method is difficult to find a suitable melt temperature during injection and obtain a proportioned polycrystal. Once the pressure difference is not properly controlled, the bubble is prone to bursting, and the red phosphorus is volatile and turns into white phosphorus when cooled during the whole process, which is dangerous. At present, this series of reasons make the synthesis of InP have the disadvantages of long synthesis time, easy explosion, low safety, and high cost. Summary of the invention
[0004] In view of the problems and shortcomings of the prior art, the present invention provides a method for vacuum synthesis of indium phosphide polycrystals, which can effectively reduce the gas phase pressure, avoid the occurrence of "tube explosion", and reduce the reaction temperature, making the material less likely to be contaminated. The whole process is short and the cost is low.
[0005] The purpose of the present invention is achieved through the following technical solutions:
[0006] A method for synthesizing indium phosphide polycrystal in vacuum, which uses indium block and red phosphorus as raw materials, mixes the raw materials according to a designed mass ratio, presses them into small pieces in a briquetting machine, puts them into a quartz tube, performs heat treatment according to a reaction temperature under vacuum conditions, and obtains a product after cooling.
[0007] The purity of the indium block and the red phosphorus powder is 99.99%.
[0008] The mass ratio of the indium block to the red phosphorus powder is 1:4-5.
[0009] The pressure of the briquetting machine to press small pieces is 3.5-4.5 MPa.
[0010] The vacuum degree of the vacuum condition is 10Pa.
[0011] The heat treatment is to raise the temperature to 650-725° C. and keep the temperature for 30-60 minutes.
[0012] The present invention is based on the formula of vapor pressure and temperature of a substance: logp (Pa) = AT -1 +BlgT+C+D, calculate the saturated vapor pressure of indium and red phosphorus under 10Pa conditions, such as Figure 1 As shown, it can be seen that the saturated vapor pressure of phosphorus does not change much with temperature; the saturated vapor pressure of indium increases with increasing temperature; but as the temperature increases, the difference in the saturated vapor pressures of indium and red phosphorus gradually decreases, which shows that vacuum conditions are conducive to the reaction of indium and phosphorus.
[0013] The present invention calculates the In-P binary equilibrium phase diagram under 10Pa conditions based on Factsage, as shown in Figure 2 As shown, the reaction temperature for generating nearly chemically matched indium phosphide is 873-1073K, and the mass ratio of indium to red phosphorus participating in the reaction is required to be 1:4-5. When more red phosphorus participates in the reaction, indium-rich indium phosphide will be generated. Therefore, under the condition of vacuum degree of 10Pa, gas-liquid reaction occurs to generate indium phosphide polycrystal, and the reaction temperature is set to 650-725°C.
[0014] The process of the present invention is short and easy to operate, and can achieve full reaction of indium and red phosphorus, and reduce the volatilization of phosphorus; because it is carried out under vacuum conditions, the reaction temperature of the raw materials is significantly reduced, and it has the advantages of economy, environmental protection, fast reaction speed, low energy consumption, etc., and the pollution is reduced in the process of generating indium phosphide, and the product quality is high, which is convenient for subsequent treatment and growth. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is the relationship diagram of the saturated vapor pressure of In and P under 10Pa conditions;
[0016] Figure 2 It is the binary equilibrium phase diagram of In and P under 10Pa condition;
[0017] Figure 3 This is the XRD pattern of the product of Example 3. DETAILED DESCRIPTION
[0018] The present invention and its specific implementation modes are further described in detail below in conjunction with the examples, but the protection scope of the present invention is not limited thereby.
[0019] Example 1
[0020] A method for vacuum synthesis of indium phosphide polycrystals, the specific steps are as follows:
[0021] (1) Raw material mixing: indium block and red phosphorus powder are weighed in a mass ratio of 1:5, and the raw materials are mixed after being weighed. The purity of the indium block and red phosphorus powder is 99.99%;
[0022] (2) briquetting of raw materials: the mixed sample obtained in step (1) is pressed into small round blocks under the condition of P≈3.5 MPa in a briquetting machine and then placed in a quartz tube for standby use;
[0023] (3) The sample obtained in step (2) was placed in an internal heating vacuum furnace, evacuated to 10 Pa, heated to 650° C. and kept warm for 60 min, and the product was taken out after cooling. The indium phosphide synthesis rate was found to be 91.3%.
[0024] Example 2
[0025] A method for vacuum synthesis of indium phosphide polycrystals, the specific steps are as follows:
[0026] (1) Raw material mixing: indium block and red phosphorus powder are weighed in a mass ratio of 1:4.5, and the raw materials are mixed after being weighed. The purity of the indium block and red phosphorus powder is 99.99%;
[0027] (2) briquetting of raw materials: the mixed sample obtained in step (1) is pressed into small round blocks under the condition of P≈4 MPa in a briquetting machine and then placed in a quartz tube for standby use;
[0028] (3) The sample obtained in step (2) was placed in an internal heating vacuum furnace, evacuated to 10 Pa, heated to 700° C. and kept warm for 35 min. The product was taken out after cooling. The indium phosphide synthesis rate was found to be 97.7%.
[0029] Example 3
[0030] A method for vacuum synthesis of indium phosphide polycrystals, the specific steps are as follows:
[0031] (1) Raw material mixing: indium block and red phosphorus powder are weighed in a mass ratio of 1:4, and the raw materials are mixed after being weighed. The purity of the indium block and red phosphorus powder is 99.99%;
[0032] (2) briquetting of raw materials: the mixed sample obtained in step (1) is pressed into small round blocks under the condition of P≈4.5 MPa in a briquetting machine and then placed in a quartz tube for standby use;
[0033] (3) The sample obtained in step (2) was placed in a horizontal tube furnace, evacuated to 10 Pa, heated to 725° C. and kept warm for 30 min, and the product was taken out after cooling. The indium phosphide synthesis rate was found to be 99.5%.
[0034] Figure 3 This is the XRD diagram of the product of step (3) of this embodiment. It can be seen from the figure that the characteristic peak of the product completely matches InP.
[0035] Comparative Example 1
[0036] After weighing the indium block and red phosphorus powder in a mass ratio of 1:5, the red phosphorus was placed at the bottom of the quartz tube, the indium block was placed at the open end of the quartz tube and a quartz block was placed, the temperature of the indium end was set to 1070°C, and the temperature of the phosphorus end was set to 500°C. After heating, the temperature was kept for 30 minutes, and the product was taken out after cooling. The indium phosphide synthesis rate was 55.4% after testing.
[0037] Comparative Example 2
[0038] (1) Raw material mixing: Indium block and red phosphorus powder are weighed in a mass ratio of 3.7:1. The raw materials are weighed and mixed. The purity of the indium block and red phosphorus powder is 99.99%;
[0039] (2) Raw material briquetting: The mixed sample obtained in step (1) is pressed into a round block under the condition of P≈4 MPa, and then placed in a quartz tube, which is sealed with a tube sealing machine;
[0040] (3) The sample obtained in step (2) was placed in a horizontal tube furnace, heated to 700° C. and kept at this temperature for 30 min. The product was taken out after cooling. The indium phosphide synthesis rate was found to be 72.0%.
[0041] In summary, the synthesis rates of indium phosphide in Examples 1-3 of the present invention are higher than those in Comparative Examples 1 and 2. In the present invention, the indium block is mixed with the red phosphorus powder and pressed into a round block, which is then placed in a quartz tube and placed in a vacuum furnace for heat treatment. The reaction temperature is lowered under vacuum conditions, all the raw materials participate in the reaction, and the synthesized product has high purity without the need for further impurity removal treatment.
Claims
1. A method for vacuum synthesis of indium phosphide polycrystals, characterized in that: The specific steps are as follows: The indium block and red phosphorus powder are mixed and pressed into a block, and then placed in a quartz tube, and heat-treated under vacuum conditions to synthesize indium phosphide polycrystals; The mass ratio of the indium block to the red phosphorus powder is 1:4-5; the vacuum degree of the vacuum condition is 10 Pa; the heat treatment temperature is 650° C.-725° C., and the insulation time is 30 min-60 min.
2. The method for vacuum synthesis of indium phosphide polycrystal according to claim 1, characterized in that: The purity of indium block and red phosphorus powder is 99.99%.
3. The method for vacuum synthesis of indium phosphide polycrystal according to claim 1, characterized in that: The briquetting pressure is 3.5~4.5MPa.
Citation Information
Patent Citations
Pressure control apparatus and method for synthesis of indium phosphide polycrystal
CN107747125A
System for preparing indium phosphide crystals by utilizing indium-phosphorus mixture
CN110760931A
Synthesis method of indium phosphide semiconductor material
CN112680790A
Direct synthesis of indium phosphide
GB2356395A
Method for producing single crystal
JP1990160687A