Chitosan-citric acid / polyvinyl alcohol double network hydrogel scaffold and preparation method and use thereof
By preparing a chitosan-citric acid/polyvinyl alcohol double network hydrogel scaffold, the problem of poor mechanical properties and rapid degradation of PVA hydrogel in cartilage repair was solved, achieving excellent mechanical properties and biocompatibility. Cartilage repair material promotes the differentiation and repair of cartilage cells.
Patent Information
- Application Number
- CN202111417476.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-25
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-11-25
AI Technical Summary
As a cartilage repair material, existing polyvinyl alcohol (PVA) hydrogel has problems such as poor mechanical properties, fragility, rapid degradation, and lack of microstructure conducive to cell adhesion, making it difficult to effectively support cartilage repair and promote cell differentiation.
The chitosan-citric acid/polyvinyl alcohol double network hydrogel scaffold is prepared through directional freezing, freeze-drying and high-temperature treatment to form a hydrogel scaffold with excellent mechanical properties and biocompatibility, providing suitable Microstructure to promote cell adhesion and differentiation.
The hydrogel scaffold has the microstructure of bionic cartilage, has mechanical properties close to normal cartilage, can effectively induce stem cells to differentiate into cartilage, has good biocompatibility and degradation properties, can be used to repair cartilage defects in knee joints in vivo, and has anti-inflammatory properties. and antibacterial effects.
Smart Images

Figure CN116159188B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of pharmaceutical chemistry, and in particular relates to a chitosan-citric acid / polyvinyl alcohol double network hydrogel scaffold and a preparation method and application thereof. Background Art
[0002] Articular cartilage is a hyaline cartilage that covers the surface of the joints. It is composed of chondrocytes and matrix. Chondrocytes account for 5% or less of the cartilage tissue. The matrix is mainly composed of proteoglycan gel and type II collagen. Proteoglycan accounts for about 35% of the dry weight of cartilage, and collagen accounts for about 60% of the dry weight of cartilage. It plays an important role in buffering stress, absorbing shock, lubricating the joint surface, and preventing wear. There are many reasons for articular cartilage damage, including acute damage caused by violent compression or tearing of the joints and chronic wear on the joints caused by long-term high-volume and high-load exercise. Studies have also shown that long-term lack of joint activity can also cause degeneration of articular cartilage. It is difficult for cartilage to repair itself after damage, so various methods for repairing articular cartilage damage have gradually been developed and applied.
[0003] Implanting a cartilage repair scaffold at the site of injury or defect is a potential method for cartilage repair. The selection of appropriate cartilage repair materials plays an important role in cartilage repair. Appropriate cartilage repair materials should have the following properties: (1) good mechanical properties to provide temporary support; 2) microstructures that are conducive to cell infiltration, adhesion, proliferation, and migration; 3) elastic modulus similar to that of the extracellular matrix of cartilage cells to facilitate the induction of stem cell differentiation into cartilage; (3) endogenous cytokine adsorption capacity to recruit endogenous cells; (3) inflammation regulation and anti-scar adhesion; (4) antibacterial and hemostatic.
[0004] In current research, polyvinyl alcohol (PVA) hydrogel is one of the preferred artificial cartilage materials due to its high water content and special surface structure, which is very similar to natural cartilage tissue. PVA hydrogel is non-toxic, stable in nature, excellent in mechanical properties, and good in hydrophilicity. At the same time, the hydrogel has a multi-microporous structure similar to natural cartilage, contains a large amount of water, and is a permeable material. Under load, liquid can penetrate and squeeze out, playing a lubricating role, greatly reducing the friction resistance to the grinding surface, and avoiding complications caused by short-term implant failure and wear debris caused by wear. However, PVA hydrogel has a low modulus when used as a cartilage repair material, cannot be used as a temporary and effective support, is difficult to degrade, and the hydrogel microstructure is not conducive to cell adhesion and lacks biological activity. Therefore, it is necessary to modify PVA hydrogel to prepare a cartilage repair material with better performance. The paper "Preparation and Performance Study of Polyvinyl Alcohol / Chitosan Porous Hydrogel" (Liu Shujing et al., Journal of Liaoning Medical College, 2013, 34(2)) discloses that a porous hydrogel for cartilage repair was prepared using polyvinyl alcohol, chitosan and polysorbate 80 as raw materials. The hydrogel has low toxicity, high water content and good cell growth and proliferation behavior; however, the hydrogel has problems such as poor mechanical properties, brittleness, rapid degradation and lack of microstructure conducive to cell proliferation and adhesion.
[0005] Therefore, further research is needed to develop a cartilage repair material that has excellent toughness, similar mechanical properties to human cartilage extracellular matrix, endogenous cell recruitment function, and anti-scarring. Summary of the invention
[0006] The purpose of the present invention is to provide a chitosan-citric acid / polyvinyl alcohol double network hydrogel scaffold and a preparation method and application thereof.
[0007] The present invention provides a chitosan-citric acid / polyvinyl alcohol double network hydrogel scaffold, which is prepared from the following raw materials in weight ratio:
[0008] 5-15 parts of polyvinyl alcohol, 5-15 parts of chitosan, and 10-30 parts of citric acid.
[0009] Furthermore, the aforementioned double network hydrogel scaffold is prepared from raw materials in the following weight ratio:
[0010] 5-15 parts of polyvinyl alcohol, 5-15 parts of chitosan, and 30 parts of citric acid.
[0011] Furthermore, the aforementioned double network hydrogel scaffold is prepared from raw materials in the following weight ratio:
[0012] 5 parts of polyvinyl alcohol, 15 parts of chitosan, and 30 parts of citric acid.
[0013] Furthermore, the double network hydrogel scaffold is obtained by preparing the above raw materials into a solution, then subjecting it to directional freezing, freeze drying, high temperature treatment, and cooling to room temperature for swelling;
[0014] The high temperature treatment is programmed temperature rise under vacuum conditions, maintaining at 80°C for 1 to 3 hours, 100°C for 1 to 3 hours, and 140°C for 1 to 3 hours; preferably, the programmed temperature rise rate is 1°C / min.
[0015] Furthermore, the solvent used to prepare the solution is double distilled water; the mass volume ratio of the polyvinyl alcohol to the solvent is 1g: (90-100)mL;
[0016] And / or, the swelling method is to immerse in PBS or physiological saline.
[0017] Furthermore, the directional freezing method is to place the solution into a mold and contact the bottom of the mold with liquid nitrogen for directional freezing;
[0018] And / or, the cooling rate is 1°C / min.
[0019] The present invention also provides a method for preparing the aforementioned double-network hydrogel scaffold, which comprises the following steps:
[0020] (1) dissolving polyvinyl alcohol, citric acid and chitosan in a solvent, removing bubbles from the solution and transferring it to a mold;
[0021] (2) placing the mold in a container filled with liquid nitrogen so that the bottom of the mold contacts the liquid nitrogen for directional freezing;
[0022] (3) freeze drying of the scaffolds obtained by directional freezing;
[0023] (4) subjecting the freeze-dried scaffold to high temperature treatment, cooling it to room temperature and then allowing it to swell;
[0024] In step (4), the high temperature treatment is programmed temperature rise under vacuum conditions, maintaining at 80°C for 1 to 3 hours, 100°C for 1 to 3 hours, and 140°C for 1 to 3 hours; preferably, the programmed temperature rise rate is 1°C / min.
[0025] Further,
[0026] In step (1), the method for eliminating bubbles is to centrifuge at 1000-2000 r / min for 5-10 minutes;
[0027] And / or, in step (2), the container is placed in an environment of 0 to 4°C;
[0028] And / or, in step (4), the cooling rate is 1°C / min;
[0029] And / or, in step (4), the swelling method is immersion in PBS or physiological saline.
[0030] The present invention also provides use of the aforementioned double-network hydrogel scaffold in preparing cartilage repair materials.
[0031] The present invention also provides a cartilage repair material, which is prepared from the aforementioned double-network hydrogel scaffold.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] 1. The prepared hydrogel scaffold has a microstructure similar to that of bionic subchondral bone plate, which is conducive to cell adhesion and proliferation.
[0034] 2. Good mechanical properties, the elastic modulus is close to the extracellular matrix of normal cartilage cells, which is conducive to inducing stem cells to differentiate into chondrocytes.
[0035] 3. It has the function of adsorbing endogenous cytokines.
[0036] 4. In vitro and in vivo experiments showed that the hydrogel scaffold has good biocompatibility, and BMSCs can grow along the pores and differentiate into chondrocytes. In vivo experiments proved that the scaffold can repair large defects in the weight-bearing area of the knee cartilage within three months.
[0037] In summary, the present invention prepares a chitosan-citric acid / polyvinyl alcohol double network hydrogel scaffold, which has good mechanical properties and a suitable degradation rate; at the same time, the hydrogel scaffold has good biocompatibility and biological activity, is non-cytotoxic, and its internal microchannel structure is conducive to stem cell adhesion, migration, and cartilage differentiation. In addition, the hydrogel scaffold has excellent anti-inflammatory and antibacterial effects and promotes cartilage regeneration when repairing cartilage in vivo, and has good application prospects in the field of tissue engineering cartilage repair.
[0038] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.
[0039] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1The gross observation, FITR, and SEM characterization results of SN hydrogel and DN hydrogel scaffolds: a is the stereoscopic microscopic images of SN and DN hydrogel scaffolds; b is the FTIR characterization spectra of SN and DN hydrogel scaffolds; c is the SEM image of the subchondral layered ECM, the SEM images of the horizontal and vertical sections of the SN hydrogel scaffold, and the SEM images of the horizontal and vertical sections of the DN hydrogel scaffold; d is the comparison of the vertical and horizontal microchannel sizes of the SN hydrogel scaffold and the DN hydrogel scaffold (n=4, *P<0.05).
[0041] Figure 2 The mechanical, swelling and degradation characterization results of SN hydrogel and DN hydrogel scaffolds: a is the compressive stress-strain curve and the corresponding Young's modulus of each hydrogel scaffold; b is the water content of each group of hydrogel scaffolds; c is the swelling characteristics of each group of hydrogel scaffolds; d is the degradation trend of each group of hydrogel scaffolds (*P<0.05, **P<0.01, ***P<0.001, ns: not significant).
[0042] Figure 3 Results of cell proliferation and cytotoxicity tests: a is live-dead staining of BMSCs cultured in scaffold extracts and normal complete medium (control) on days 1, 3, and 5; b is quantitative analysis of cell viability; c is cytotoxicity determination by CCK-8 test on days 1, 3, and 5 (ns: not significant).
[0043] Figure 4 The morphology of BMSCs after co-culture with the hydrogel scaffold: the black and white picture on the left is the morphology of BMSCs on the scaffold analyzed by SEM; the color picture on the right is the rhodamine-coupled phalloidin-stained cytoskeleton of BMSCs analyzed by fluorescence microscopy, red represents the cytoskeleton, and blue represents the cell nucleus.
[0044] Figure 5 The results of in vitro chondrogenic differentiation of BMSCs on the scaffold; a is the relative mRNA expression of chondrogenic specific markers (CollagenⅡ, Aggrecan, Sox9) analyzed by RT-qPCR at the 2nd and 3rd weeks; b is the protein expression of CollagenⅡ, Aggrecan, and Sox9 detected by Western blot at the 3rd week; c is the expression of collagenⅡ, Aggrecan, and Sox9 detected by immunofluorescence at the 3rd week, yellow indicates target protein, and blue indicates cell nucleus (*P<0.05, **P<0.01***P<0.001).
[0045] Figure 6The gross and histological analysis of the joint defect sites 4, 8 and 12 weeks after surgery: a is a gross photograph of the defect sites in the scaffold group and the control group, the yellow circle indicates the defect site, and the red arrow indicates the collapse of the osteochondral tissue around the defect in the control group; b is the evaluation of the regeneration effect using ICRS and OAS scores.
[0046] Figure 7 Histological analysis of joint defect sites 4, 8, and 12 weeks after surgery: H&E, Safranin-O / FastGreen, and Alcian Blue (AB) staining were used to evaluate the new tissue.
[0047] Figure 8 IHC analysis of neonatal tissue 4, 8, and 12 weeks after surgery: detection of COL II, aggrecan, and Sox-9. DETAILED DESCRIPTION
[0048] The raw materials and equipment used in the specific embodiments of the present invention are all known products and are obtained by purchasing commercially available products.
[0049] Example 1. Preparation of the hydrogel scaffold of the present invention
[0050] The method for preparing the double network (DN) hydrogel scaffold is as follows:
[0051] In a 90°C water bath and 100r / min stirring condition, 0.5g polyvinyl alcohol (PVA) was dissolved in 48mL double distilled water (ddH2O) to obtain a transparent solution cooled to room temperature. 3g citric acid was dissolved in the above transparent solution, and then 1.5g chitosan was added to the solution under vigorous stirring. The bubbles in the solution were eliminated by centrifugation at 2000r / min for 5 minutes, and the obtained solution was transferred to a customized cylindrical polytetrafluoroethylene mold (d=30mm, h=50mm) with thick walls (3mm) and thin bottom (1mm). An insulated container filled with liquid nitrogen was used as a cold source for the directional freezing process. The polytetrafluoroethylene mold containing the solution was placed on the top of the insulated container, and the entire device was placed in an environment of 4°C. The solution was directionally frozen. After about 1.5h, the obtained frozen scaffold was freeze-dried, and a freeze-dried snow-white cylindrical scaffold was obtained after 72 hours. Subsequently, the snow-white cylindrical scaffold was transferred to a vacuum oven, and after evacuation, the temperature was programmed to rise (80°C for 1 h, 100°C for 1 h, 140°C for 1 h, and the heating rate was 1°C / min). Then, the system was gradually cooled to room temperature (cooling rate was 1°C / min) to obtain a light yellow cylindrical scaffold. Finally, the scaffold was immersed in an appropriate amount of PBS (Gibco, Shanghai, China), and the pH was adjusted to 7.35-7.45 with NaHCO3 (1 mol / L). The DN hydrogel scaffold was obtained.
[0052] Different DN hydrogel scaffolds were prepared by changing the mass ratio of chitosan and polyvinyl alcohol. The above 1.5 g chitosan, 0.5 g polyvinyl alcohol (the mass ratio of chitosan to PVA was 1.5 / 0.5, w / w) was changed to: 1.5 g chitosan, 1.5 g polyvinyl alcohol (the mass ratio of chitosan to PVA was 1.5 / 1.5, w / w), 1.5 g chitosan, 1.0 g polyvinyl alcohol (the mass ratio of chitosan to PVA was 1.5 / 1.0, w / w), 1.0 g chitosan, 1.0 g polyvinyl alcohol (the mass ratio of chitosan to PVA was 1.0 / 1.0, w / w), 1.0 g chitosan, 0.5 g polyvinyl alcohol (the mass ratio of chitosan to PVA was 1.0 / 0.5, w / w), 0.5 g chitosan, 0.5 g polyvinyl alcohol (the mass ratio of chitosan to PVA was 0.5 / 0.5, w / w).
[0053] Comparative Example 1: Preparation of Single Network (SN) Hydrogel Scaffold
[0054] 3 g of citric acid was dissolved in 48 mL of double distilled water (ddH2O), and then 1.5 g of chitosan was added to the solution under vigorous stirring. The solution was centrifuged at 2000 r / min for 5 minutes to eliminate bubbles in the solution, and the obtained solution was transferred to a custom cylindrical polytetrafluoroethylene mold (d = 30 mm, h = 50 mm) with thick walls (3 mm) and thin bottoms (1 mm). An insulated container filled with liquid nitrogen was used as a cold source for the directional freezing process. The polytetrafluoroethylene mold containing the solution was placed on the top of the insulated container, and the entire device was placed in an environment of 4°C. The solution was directional frozen. After about 1.5 hours, the obtained frozen scaffold was freeze-dried, and the freeze-dried cylindrical scaffold was obtained after 72 hours. Subsequently, the cylindrical scaffold was transferred to a vacuum oven, and a temperature program was started after vacuuming (80°C for 1 hour, 100°C for 1 hour, 140°C for 1 hour, and the heating rate was 1°C / min). Then, the system was gradually cooled to room temperature (cooling rate was 1°C / min) to obtain the scaffold. Finally, the scaffold was immersed in an appropriate amount of PBS (Gibco, Shanghai, China), and the pH was adjusted to 7.35-7.45 with NaHCO3 (1 mol / L), thereby obtaining a single network (SN) hydrogel scaffold.
[0055] Different SN hydrogel scaffolds were prepared by changing the amount of chitosan used. The chitosan amounts were 1.5 g, 1.0 g, and 0.5 g, respectively.
[0056] The beneficial effects of the present invention are demonstrated below through specific test examples.
[0057] The macroscopic morphology of the DN hydrogel scaffold and the SN hydrogel scaffold prepared in the examples and comparative examples is shown in FIG. Figure 1As shown in a; including the front view and top view of the drying scaffold, as well as the front view and top view after swelling the scaffold in PBS.
[0058] Unless otherwise specified, the double-network hydrogel scaffolds (DN hydrogel scaffolds) in the following test examples are all hydrogel scaffolds prepared using 1.5 g of chitosan and 0.5 g of polyvinyl alcohol in Example 1; the single-network hydrogel scaffolds (SN hydrogel scaffolds) are all hydrogel scaffolds prepared using 1.5 g of chitosan in Comparative Example 1.
[0059] Statistical analysis
[0060] All quantitative data are reported in the form of mean ± standard deviation. Statistical analysis was performed using the SPSS 25.0 statistical software package. Unpaired Student's t-tests were used to compare the groups. Values of p < 0.05 were considered statistically significant. Data are indicated by (*) for 0.01 < p < 0.05, (**) for 0.001 < p ≤ 0.01, and (***) for p ≤ 0.001.
[0061] Test Example 1, FTIR characterization of the hydrogel scaffold of the present invention
[0062] The hydrogel scaffold prepared by the present invention was characterized by an FTIR spectrometer (Thermo Scientific Nicolet iS50 FTIR) to identify the functional groups of the scaffold and confirm the amidation of chitosan. Tablets were prepared using KBr for characterization, with air as the background control.
[0063] The results are as Figure 1 shown in b, Figure 1 In b, CS1.5-HT is a SN hydrogel scaffold, CS1.5-PVA0.5-HT is a hydrogel scaffold prepared using 1.5 g of chitosan and 0.5 g of polyvinyl alcohol in Example 1, and CS1.5-PVA1.5-HT is a hydrogel scaffold prepared using 1.5 g of chitosan and 1.5 g of polyvinyl alcohol in Example 1. From Figure 1 b, it can be seen that the characteristic peaks at 3500 cm -1 , 1638 cm -1 and 1540 cm -1 correspond to the blending of N-H and O-H, C=O, and N-H, respectively. This indicates that the hydrogel scaffold of the present invention was successfully prepared.
[0064] Test Example 2, SEM images of the hydrogel scaffold of the present invention
[0065] Scanning electron microscope (Nova NanoSEM450) was used to observe decalcified rat subchondral bone slices, horizontal slices and vertical slices of the DN hydrogel scaffold of the present invention, and horizontal slices and vertical slices of the SN hydrogel scaffold. The size was measured using Image J.
[0066] The results are as follows Figure 1 As shown in c, Figure 1 c It can be seen that the double network hydrogel scaffold has microchannels similar to natural subchondral bone, and the pore wall has step-like stripes similar to the pore wall of natural subchondral bone channel (as indicated by the arrow). The single network hydrogel scaffold has similar pores, but the pore wall is smooth and has no step-like stripes. The results show that the double network hydrogel scaffold constructed by the present invention has a microstructure and morphology similar to the extracellular matrix of subchondral bone.
[0067] Figure 1 d is the microchannel size of the single-network hydrogel scaffold and the double-network hydrogel scaffold, indicating that the hydrogel scaffold prepared by the present invention has a microchannel structure of appropriate size suitable for cell growth.
[0068] Test Example 3: Mechanical properties test of the hydrogel scaffold of the present invention
[0069] The compression test uses a sample with a height of 50 mm and a diameter of 30 mm. After complete swelling at 37 ° C in PBS, a compressive stress-strain test is performed in an atmosphere of 37 ° C using an Instron general instrument (Instron 5567) equipped with a 100 kN sensor. The compression rate is maintained at 5 mm / min. The strain of each compression process is set to 85%. All tests are repeated 3 times. The compression Young's modulus includes an approximate linear fit value under 10-15% strain deformation.
[0070] The results are as follows Figure 2 As shown in a, Figure 2 a It can be seen that the double network hydrogel scaffold can withstand 85% deformation and remain intact. The single network hydrogel scaffold is relatively fragile. And it can be seen that the elastic modulus of the double network hydrogel scaffold is about 0.26MPa, which is significantly higher than the elastic modulus of the single network hydrogel scaffold and close to the elastic modulus of the natural cartilage extracellular matrix. It shows that the constructed DN hydrogel scaffold has perfect mechanical properties for cartilage repair. It can withstand the required deformation, and the modulus is similar to that of natural cartilage. It can effectively transmit mechanical signals, which is conducive to inducing stem cells to differentiate into chondrocytes.
[0071] Experimental Example 4: Swelling and degradation characteristics of the hydrogel scaffold of the present invention
[0072] The dried scaffolds were weighed and then immersed in PBS. When the scaffolds were fully swollen, the weight of the scaffolds was measured and recorded. The swollen scaffolds were then placed on a shaker (37°C, 100r / min). PBS was changed once a week. At each time point, the remaining scaffolds were freeze-dried and the weight was measured. The weight of the dry sample at a fixed time point was recorded as Wt, and the initial dry weight was recorded as W0. There were four replicates (n=4) in each group.
[0073] After the scaffold is fully swollen. The weight is recorded as Ws. Water absorption (Ww) = Ws-W0. The water ratio in the swollen hydrogel scaffold is calculated as Ww% = Ww / Ws*100%. The increased height and diameter are measured after full swelling and recorded as Ds and Hs, respectively. The initial diameter and height are measured and recorded as Di and Hi, respectively. The increased diameter is calculated as the increased diameter (%) = (Ds-Di) / Di*100%. The increased height is calculated as the increased height (%) = (Hs-Hi) / Hi*100%.
[0074] The residual mass of the scaffold at each time point was calculated as residual mass (%) = (Wt-W0) / W0*100%.
[0075] The results are as follows Figure 2 As shown in b-2d, it can be seen from the figure that the SN hydrogel scaffold is basically completely degraded within 3 months, while the DN hydrogel scaffold is basically completely degraded within 6 months. The degradation rate of the DN hydrogel scaffold is significantly slower than that of the SN hydrogel scaffold. It shows that the DN hydrogel scaffold of the present invention has a degradation performance suitable for cartilage repair, can provide support for a sufficiently long time, and can gradually degrade while the cartilage regenerates.
[0076] Experimental Example 5: Cytotoxicity test of the hydrogel scaffold of the present invention
[0077] The biocompatibility of the control group (Petri dish) and DN hydrogel scaffolds (CS1.5-PVA0.5) was evaluated using a live / dead staining kit (Solarbio, Beijing, China) and a cell CCK-8 kit (Solarbio, Beijing, China). Before the in vitro experiment, the scaffolds were sterilized by ethylene oxide gas method (1200 mg / L, 37°C, 6 hours), and the sterilization indicator strip was packaged together with the scaffolds to confirm the sterilization qualification. Then, the scaffold extract was prepared. In brief, 2 g of scaffolds were immersed in complete culture medium and cultured at 37°C for 24 hours to obtain the extract. 1000 BMSCs were resuspended in 96-well culture plates with 100 μl of the above extract (scaffold group) or normal complete culture medium (control group). Three replicate samples were collected for each group at each time point.
[0078] After 1, 3, and 5 days of culture, CCK-8 (10 μl per group) was added to each group. After incubation at 37°C for 2 hours, the optical density was measured at 450 nm and the cell viability was calculated. The absorbance of cells cultured in the extraction medium and normal medium was used as OD Scaffold and OD 对照 .
[0079] A mixed solution containing Calcein-AM and propidium iodide (PI) was added to the samples and incubated at 37°C for 30 minutes. Live (green) / dead (red) staining of cells in extracts or normal culture medium was then observed under an inverted fluorescence microscope (Olympus IX83). Cell proliferation was analyzed on days 1, 3, and 5.
[0080] The results are as follows Figure 3 As shown in Figure 3, it can be seen that the hydrogel scaffold of the present invention has no cytotoxicity.
[0081] Experimental Example 6: Effect of the hydrogel scaffold of the present invention on cell morphology and adhesion
[0082] F-actin fluorescence staining was used to evaluate the morphology of BMSCs cultured in scaffold extracts. After culturing for 1, 3, and 5 days as described in Experimental Example 5, the cells were washed with PBS and fixed with 4% (W / V) neutral paraformaldehyde for 30 minutes. F-actin was stained with rhodamine-conjugated phalloidin (Solarbio, Beijing, China). The nuclei were stained with 4,6-diami-dino-2-phenylindole (DAPI, Solarbio, Beijing, China). After washing with PBS three times, the cell morphology was observed under a fluorescence microscope (NI-E, Nikon, Tokyo, Japan) at an excitation wavelength of 405 nm (DAPI) and an emission wavelength of 561 nm (rhodamine-conjugated phalloidin).
[0083] To further evaluate whether BMSCs would migrate into the scaffold through the microchannels. 20,000 BMSCs were seeded in a 6-well plate. After 24 hours of culture, the prepared cylindrical scaffold (diameter: 10 mm, height: 5 mm) was placed in the BMSCs in the seeding well. After 5 days of culture, the scaffold was fixed with 4% (W / V) neutral paraformaldehyde for 30 minutes and dehydrated with graded ethanol. The samples were then dried under vacuum for 6 hours and subsequently observed under a scanning electron microscope (Nova NanoSEM450).
[0084] The results are as follows Figure 4 As shown in the figure, it can be seen that BMSCs are in an adherent state on the scaffold, and BMSCs can migrate into the scaffold through the microchannel. It shows that the hydrogel scaffold does not affect the adhesion and migration of stem cells, and its microchannel structure is conducive to the adhesion and migration of stem cells into the scaffold.
[0085] Experimental Example 7: In vitro cartilage differentiation
[0086] BMSCs were seeded in the double network hydrogel scaffold (CS1.5-PVA0.5) of the present invention and co-cultured in chondrogenic medium (Cyagen, Guangzhou, China) in a humidified atmosphere of 5% CO2 at 37°C. The medium was replaced every 3 days. The expression of type II collagen, aggrecan, and Sox9 was analyzed by real-time quantitative PCR at the 2nd and 3rd weeks of culture. At the 3rd week, the expression of CollagenⅡ, Aggrecan, and Sox9 was further detected by Western-Blot and immunofluorescence.
[0087] Quantitative real-time polymerase chain reaction (RT-qPCR)
[0088] Gene expression analysis was performed by RT-qPCR after 14 and 21 days of culture (n=3). For hydrogel structures, samples were collected and mechanically ground in liquid nitrogen. Total cellular RNA was extracted using Trizol reagent (Tiangen, Beijing, China) and reversely transcribed into cDNA using a kit (Thermo Fisher, Shanghai, China). RT-qPCR was performed using a real-time qPCR system (Biorad CFX 96) to evaluate the expression of cartilage-related markers, including Col II, Aggrecan, SOX9, and the housekeeping gene GAPDH was used for standardization. The final results of relative gene expression were determined using the ΔΔCt method.
[0089] Western blot (WB) analysis
[0090] Protein expression levels were detected by WB after 21 days of culture. Total proteins were extracted, separated by sodium dodecyl sulfate-polyacrylamide gel electrophoresis (SDS-PAGE) and transferred to polyvinylidene difluoride membranes, which were incubated with primary antibodies against Col II (#33340, Signalway Antibody, USA), Aggrecan (#45068, Signalway Antibody, USA) and SOX9 (#49070, Signalway Antibody, USA) at 4°C overnight. After washing, the membranes were incubated with horseradish peroxidase-conjugated secondary antibodies (1:5000 dilution) at room temperature for 1 hour, and the membranes were treated with enhanced luminol detection reagent (Santa Cruz Biotechnology, USA) before exposure. The gray value of β-actin was used for reference.
[0091] Immunofluorescence
[0092] The prepared BMSCs scaffolds were cultured in chondrogenic medium for 21 days. After gently washing with PBS, the constructs were fixed in 4% paraformaldehyde for 30 minutes. Subsequently, the constructs were frozen in liquid nitrogen and cut into 3 μm slices. The slices were blocked with 5% BSA. Then, the slices were incubated with primary antibodies of Col II (#33340, Signalway Antibody, USA), Aggrecan (#45068, Signalway Antibody, USA) and SOX9 (#49070, Signalway Antibody, USA) at 4 ° C overnight. After rewarming the next day, the slices were incubated with rhodamine-conjugated goat anti-rat IgG secondary antibodies (Jackson ImmunoResearch, USA), and the cell nuclei were visualized with 4',6-diamidino-2-phenylindole (DAPI, Solarbio, Beijing, China) All slices were observed by fluorescence microscopy (Nikon Ni-E).
[0093] The results are as follows Figure 5 As shown in the figure, it can be seen that BMSC can differentiate into cartilage on the synthesized scaffold. It is shown that the scaffold does not affect the differentiation of stem cells into chondrocytes.
[0094] Test Example 8: In vivo regeneration of cartilage
[0095] All SD rats used in this study were operated in accordance with the guidelines approved by the Ethics Committee of West China Hospital, Sichuan University (20211169A). A full-thickness cartilage defect model was created in 18 (n=9 per group) 12-week-old SD rats (2.5-3.0 kg) to evaluate the repair effect of the DN hydrogel scaffold (CS1.5-PVA0.5). The rats were housed individually in cages and anesthetized with pentobarbital (W / V 1.5%). The disinfection procedure was completed. Subsequently, an osteochondral defect (diameter: 2.0 mm, depth: 3 mm) was created in the load-bearing area adjacent to the femoral attachment of the anterior cruciate ligament so that most of the early cartilage defects could be observed in this area. The experimental group implanted the prepared scaffold into the defect. The blank control group was not treated. Both hind knees were involved in the surgery. After the operation, no activity restrictions were imposed on any animal. No antibiotics were used to prevent infection. Rats were killed by intraperitoneal injection of an overdose of pentobarbital (W / V 1.5%) at 4, 8, and 12 weeks after surgery, and the knee joints were removed for gross observation and histological analysis. Subsequently, macroscopic evaluation was used to evaluate the regenerated tissue. In addition, hematoxylin and eosin (HE), safranin-O / Fast Green, and Alcian Blue (AB) were used to stain the specimens of each group to further study the regeneration effect. In addition, immunohistochemistry was used to observe the expression of CollagenⅡ, Aggrecan, and Sox9, and the evaluation was performed under a microscope (Nikon, Ni-E).
[0096] Macroscopic and histological findings were analyzed by 3 investigators blinded to the groups. The International Cartilage Repair Society (ICRS) score and Oswestry arthroscopic score (OAS) were assessed.
[0097] The results are as follows Figure 6 As shown in a, it can be seen from the figure that compared with the control group, in general, 4 weeks after implantation, the defects implanted with DN hydrogel scaffolds were filled with fresh soft tissue, but still not remodeled. No cartilage wear and osteochondral collapse were found in the joints implanted with DN hydrogel scaffolds. In addition, no immune rejection or synovial proliferation was observed in the DN hydrogel scaffold group. However, the defects in the control group were filled with thin fibrous tissue, which was irregular and clearly distinguished from the surrounding cartilage. In addition, wear of the surrounding cartilage and osteochondral collapse around the defect were observed in the control group.
[0098] Eight weeks after implantation, the defects in the DN hydrogel scaffold group were filled with more mature and remodeled tissue, similar to natural cartilage. However, in the control group, the defects were filled with more fibrous tissue. The collapsed areas were also replaced by fibrous tissue.
[0099] After 12 weeks of implantation, the DN hydrogel scaffolds significantly repaired the cartilage defects ( Figure 7 ). However, in the control group, severe arthritis, defects, and surrounding collapse replaced by fibrous tissue were observed.
[0100] Figure 6 b is the ICRS and OAS evaluation results. It can be seen from the figure that the ICRS and OAS scores of the DN hydrogel scaffold group were significantly higher than those of the control group, indicating that the DN hydrogel scaffold of the present invention has a good effect on cartilage regeneration.
[0101] Gross visualization may not fully reflect the maturity of the new tissue. To make a more thorough assessment of the situation, histology and IHC analysis were performed to further analyze the new tissue. The decalcified femoral sites of the knee joint at 4, 8, and 12 weeks after surgery involved hematoxylin and eosin (H&E), Safranin-O (Saf-O) / Fast Green, and Alcian Blue (AB) staining. To evaluate the in vivo expression of cartilage-specific markers in the new tissue, COL II, aggrecan (Agg), and Sox-9 were detected by IHC analysis.
[0102] from Figure 7H&E staining showed that the defects in the DN hydrogel group were filled with uniform and smooth regenerated tissue. At 4 weeks after implantation, the new tissue resembled cartilage-like tissue. Over time, until 8 and 12 weeks after surgery, the new tissue became more and more mature and formed cartilage-like tissue. In contrast, in the control group, the defects were filled with thin fibrous tissue at 4 weeks, with almost no cartilage-like tissue. Over time, at 8 and 12 weeks after surgery, more and more fibrous tissue was found in the defects, but very little cartilage-like tissue was still found.
[0103] Safranin-O / Fast Green and Alcian Blue staining are used to better distinguish the cartilage tissue components in the new tissue. Safranin-O will stain the cartilage tissue red, while Fast Green will stain the bone tissue green. Alcian Blue will specifically stain the cartilage tissue blue. Figure 7 As shown, at 4 weeks, a small amount of cartilage tissue was found in the defect of the DN hydrogel scaffold group. As time went on, more and more cartilage tissue was found in the defect. At 12 weeks after surgery, the defect was almost filled with cartilage tissue. In the control group, very little cartilage tissue was found in the defect at all 3 time points.
[0104] In addition, IHC analysis was used to analyze cartage-specific markers, including collagen II, aggrecan (Agg), and Sox9. Figure 8 As shown, the regenerated cartilage in the DN hydrogel scaffold group showed more collagen II, aggrecan, and Sox9 on the ECM. In addition, the cells in the DN hydrogel scaffold group maintained their morphology and arranged vertically in columns, which is similar to that in native cartilage. In the DN hydrogel scaffold group, the bone tissue in the deeper part was also remodeled. Compared with the DN hydrogel group, the expression of cartilage-specific markers was poor and the surface was more irregular.
[0105] The experimental results show that the DN hydrogel scaffold has great potential to promote cartilage regeneration in the load-bearing area of the joint from several aspects: 1) Providing temporary mechanical support for the tissue around the defect to avoid the collapse of the surrounding osteochondral tissue. 2) Infiltration, attachment, proliferation, migration of endogenous cells and promoting cartilage differentiation. 3) Avoiding defective fiber replacement.
[0106] In summary, the present invention prepares a chitosan-citric acid / polyvinyl alcohol double network hydrogel scaffold, which has good mechanical properties and a suitable degradation rate; at the same time, the hydrogel scaffold has good biocompatibility and biological activity, is non-cytotoxic, and its internal microchannel structure is conducive to stem cell adhesion, migration, and cartilage differentiation. In addition, the hydrogel scaffold has excellent anti-inflammatory and antibacterial effects and promotes cartilage regeneration when repairing cartilage in vivo, and has good application prospects in the field of tissue engineering cartilage repair.
Claims
1. A chitosan-citric acid / polyvinyl alcohol double network hydrogel scaffold, Features: It is prepared from the following raw materials in the following weight ratio: 5 parts of polyvinyl alcohol, 15 parts of chitosan, 30 parts of citric acid; The double network hydrogel scaffold is prepared by preparing the above raw materials into a solution, and then subjecting it to directional freezing, freeze drying, high temperature treatment, and cooling to room temperature for swelling; The high temperature treatment is programmed heating under vacuum conditions, maintaining at 80° C. for 1 to 3 hours, 100° C. for 1 to 3 hours, and 140° C. for 1 to 3 hours.
2. The double network hydrogel scaffold according to claim 1, Features: The solvent used to prepare the solution is double distilled water; the mass volume ratio of the polyvinyl alcohol to the solvent is 1g: (90-100)mL; And / or, the swelling method is to immerse in PBS or physiological saline.
3. The double network hydrogel scaffold according to claim 1, Features: The programmed temperature rise rate is 1°C / min.
4. The double network hydrogel scaffold according to claim 1, Features: The method of directional freezing is to place the solution into a mold and contact the bottom of the mold with liquid nitrogen for directional freezing; And / or, the cooling rate is 1°C / min.
5. A method for preparing the double network hydrogel scaffold according to any one of claims 1 to 4, Features: It includes the following steps: (1) dissolving polyvinyl alcohol, citric acid and chitosan in a solvent, removing bubbles from the solution and transferring it to a mold; (2) placing the mold in a container filled with liquid nitrogen so that the bottom of the mold contacts the liquid nitrogen for directional freezing; (3) freeze drying of the scaffolds obtained by directional freezing; (4) subjecting the freeze-dried scaffold to high temperature treatment, cooling it to room temperature and then allowing it to swell; In step (4), the high temperature treatment is programmed temperature rise under vacuum conditions, maintaining at 80°C for 1 to 3 hours, 100°C for 1 to 3 hours, and 140°C for 1 to 3 hours; preferably, the programmed temperature rise rate is 1°C / min.
6. The method according to claim 5, Features: In step (1), the method for eliminating bubbles is to centrifuge at 1000-2000 r / min for 5-10 minutes; And / or, in step (2), the container is placed in an environment of 0 to 4°C; And / or, in step (4), the cooling rate is 1°C / min; And / or, in step (4), the swelling method is immersion in PBS or physiological saline.
7. Use of the double network hydrogel scaffold according to any one of claims 1 to 4 in the preparation of cartilage repair materials.
8. A cartilage repair material, Features: It is prepared from the double network hydrogel scaffold described in any one of claims 1 to 4.