A composite catalytic material containing all-silicon molecular sieve and its preparation method and application
By adding metal precursors, polyhydroxyl auxiliaries and silanization reagents during the synthesis process of molecular sieves, composite catalytic materials of metal nanoparticles and molecular sieves are prepared, which solves the problem of insufficient catalytic activity in the existing technology and achieves high levels of metal nanoparticles. The formation of dispersion and hierarchical pore structure significantly improves the catalytic activity.
Patent Information
- Application Number
- CN202111424550.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-11-26
AI Technical Summary
It is difficult to simultaneously achieve high dispersion of metal nanoparticles and preparation of hierarchical pore molecular sieves in the same preparation method with the existing technology, resulting in insufficient catalytic activity.
By adding metal precursors, polyhydroxyl auxiliaries and silanization reagents during the synthesis process of molecular sieves, and performing hydrothermal crystallization and roasting treatments, composite catalytic materials of metal nanoparticles and molecular sieves are prepared to achieve highly dispersed and multi-level metal nanoparticles. Formation of pore structure.
A composite catalytic material of metal nanoparticles and molecular sieves with large specific surface area, pore volume and high catalytic activity was obtained, especially showing high catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.
Smart Images

Figure CN116174018B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of catalytic materials, and in particular, to a composite catalytic material containing an all-silicon molecular sieve, and a preparation method and application thereof. Background Art
[0002] Generally speaking, it is difficult to highly disperse metal nanoparticles into molecular sieve crystals using conventional impregnation methods. This is because the micropore size of the molecular sieve is small, and the impregnation method usually uses metal salt solutions for impregnation. The size of metal hydrated ions is generally larger than the pore size of the molecular sieve and cannot diffuse into the pores, so they can only gather on the outer surface of the molecular sieve particles. In order to solve this problem, researchers have developed two series of preparation methods: direct synthesis and post-synthesis. The direct synthesis method generally refers to the direct introduction of metal precursors during the crystallization process of the molecular sieve. During the hydrothermal crystallization process, the metal precursor can interact with the secondary structure of the molecular sieve through electrostatic effects or van der Waals forces. Therefore, during the self-assembly process of the secondary structural units, the metal nanoparticles are evenly embedded in the molecular sieve skeleton.
[0003] Conventional microporous molecular sieves can only be diffused by reactants of small molecular size due to pore restrictions, and thus cannot catalyze reactions involving macromolecular substrates. In view of this defect, mesopores or even macropores are introduced into microporous molecular sieves to construct molecular sieves with multi-level pore sizes, thereby improving the performance of microporous molecular sieves when applied to macromolecular reactants. According to different synthesis methods, the synthesis methods of multi-level pore molecular sieves mainly include skeleton atom removal method, double template synthesis method ordered micro-mesoporous composite molecular sieve, hard template method, dry gel conversion method and silanization method. Among them, silanization method is a relatively simple and widely used method. Since the silanol of the silanization agent and the silanol of the molecular sieve precursor are hydrolyzed and condensed to produce a stable Si-O-Si bond, the realization of the supporting layer pore expansion effect is ensured. For example, Wang Baorong et al. (CN111847471A) prepared a multi-level pore molecular sieve encapsulating active metals by introducing a silanization agent in a direct hydrothermal synthesis method. However, since the above process is carried out under strong alkalinity and high temperature hydrothermal conditions, the metal precursor is very easy to form hydroxide precipitation. In order to solve this problem, the precursor metal ions often form complexes with ligands containing lone pair electrons (such as organic amine ligands or ammonia). For example, Wang et al. used ethylenediamine ligands to form complexes with PdCl 2 Formation of [Pd(NH 2 CH 2 CH 2 NH 2 )]Cl 2The complex precursor was then directly synthesized by hydrothermal crystallization to embed and disperse Pd nanoparticles in silicalite-1 molecular sieve (Pd@silicalite-1). Using ligands to strengthen the stability and dispersion of metals is an important means to prepare metal nanoparticles and molecular sieve composite catalytic materials. Polyhydroxy compounds, such as polyols such as glycerol, and polyhydroxy sugars, contain multiple hydroxyl groups, have good coordination and protection effects on metal ions, and can form good mutual solubility with water. In summary, although the metal precursor is complexed with an organic ligand and then introduced into the molecular sieve hydrothermal crystallization process, the metal nanoparticles can be highly dispersed in the molecular sieve crystal; the introduction of silanization agents into the molecular sieve synthesis process can also effectively and simply prepare multi-level pore molecular sieves. However, in general research, it is difficult to achieve the above two purposes at the same time in the same preparation method to obtain a molecular sieve with the advantages of both, that is, it is difficult to directly prepare a multi-level pore molecular sieve with highly dispersed metal nanoparticles. Summary of the invention
[0004] The purpose of the present disclosure is to provide a composite catalytic material containing all-silicon molecular sieves and a preparation method and application thereof. The composite catalytic material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the metal oxide particles have a uniform particle size and have a high dispersion in the molecular sieve crystal and on the pore surface.
[0005] In order to achieve the above-mentioned object, the first aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material, comprising an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the composite catalytic material has the following UV-Vis characteristics: in the peak separation result of the wavelength of 450 to 740 nm in the UV-Vis spectrum of the composite catalytic material, the peak area of the spectrum peak in the wavelength range of 650 to 670 nm is recorded as A 1 The total peak area in the wavelength range of 450 to 740 nm in the UV-Vis spectrum of the composite catalyst material is recorded as A 2 , A defined by the following formula (1) 0 Any value between 0.4 and 0.6; A 0 =A 1 / A 2 Formula (1).
[0006] Optionally, the A 0 The value of is any value between 0.45 and 0.6.
[0007] Optionally, the all-silicon molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve;
[0008] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.
[0009] Optionally, in the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.2):1, preferably (0.001-0.18):1.
[0010] Optionally, the BET specific surface area of the composite catalytic material is 400 to 800 m 2 / g, the total pore volume is 0.3-0.65mL / g, the micropore volume is 0.1-0.19mL / g, the mesopore volume is 0.2-0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-8nm.
[0011] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nanoparticles and molecular sieves, comprising the following steps:
[0012] S1, mixing a template, a silicon source, water, a metal M precursor, a polyhydroxy auxiliary and a silanization agent to obtain a reaction mixture; wherein the polyhydroxy auxiliary is a compound containing at least two hydroxyl groups; and the silanization agent contains at least one coordination group capable of complexing with the metal element M;
[0013] S2. performing hydrothermal crystallization and calcination on the reaction mixture.
[0014] Optionally, in step S1, SiO 2 The molar ratio of silicon source: template: water: metal element M: silanization agent is 1: (0.005-1): (10-80): (0.001-0.2): (0.025-0.4), preferably 1: (0.005-1): (10-80): (0.001-0.18): (0.025-0.3); the molar ratio of polyhydroxy auxiliary agent to metal element M is (0.2-2): 1, preferably (0.5-2): 1.
[0015] Optionally, step S1 includes:
[0016] a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution;
[0017] b. Adding a polyhydroxy auxiliary agent to an aqueous solution of a metal M precursor, and mixing the mixture to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material;
[0018] c. Adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture; preferably, the mixing conditions in step c include: stirring at 20 to 80° C. for 0.5 to 2 hours.
[0019] Optionally, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably selected from at least one of organic silicone grease, solid silica gel and white carbon black; further preferably organic silicone grease, the general formula of the organic silicone grease is the structure shown in the following formula (A):
[0020]
[0021] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl; further preferably, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0022] Optionally, in step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;
[0023] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.
[0024] Optionally, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines; further preferably, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):
[0025] R 1 , R 2 , R 3 and R 4 are independently selected from an alkyl group having 1 to 4 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms, more preferably R 1 , R 2 , R 3 and R 4 Each of the following is selected from the group consisting of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl;
[0026] Further preferably, the molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0027] The molecular sieve of the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0028] The molecular sieve of the composite catalytic material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
[0029] Optionally, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;
[0030] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0031] Preferably, the metal M precursor is an aqueous solution of the metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0032] Optionally, in step S1, the polyhydroxy auxiliary agent is selected from one or more of polyols and sugar substances;
[0033] Preferably, the polyol comprises one or more of ethylene glycol, glycerol, pentaerythritol, 1,2-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, neopentyl glycol, diethylene glycol and polyether polyol; wherein the polyether polyol comprises one or more of propylene glycol polyether, trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol; the weight average molecular weight of the propylene glycol polyether is 800-2000, and the weight average molecular weight of the trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol is independently 400-4000;
[0034] The sugar substances include one or more of glucose, sucrose, fructose, starch and cellulose.
[0035] Optionally, in step S1, the general formula of the silanization agent is R 5 Si(R 6 )(R 7 )R 8 , where R 5 , R 6 , R 7 , R 8 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R 5 , R 6 , R 7 , R 8 At least one of them is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the alkyl group, the alkoxy group, the thiol group and the amine group each independently have 1 to 18 carbon atoms, and the aromatic group has 6 to 18 carbon atoms;
[0036] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0037] Optionally, in step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.;
[0038] The conditions for the calcination treatment include: a calcination temperature of 400 to 900° C. and a calcination time of 1 to 16 hours; preferably, the calcination temperature is 400 to 800° C. and the calcination time is 2 to 8 hours.
[0039] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.
[0040] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0041] Through the above technical scheme, the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material and its preparation method and application. The present disclosure adds a metal precursor, a polyhydroxy auxiliary agent and a silanization agent to the reaction raw materials of the molecular sieve crystallization synthesis, and the molecular sieve of the composite catalytic material prepared has a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal oxide nanoparticles have uniform particle size and are evenly dispersed in the mesoporous channels of the multi-level pore molecular sieve; the composite catalytic material has high catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0042] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0044] Figure 1 This is the UV-Vis spectrum of the product prepared in Example 1.
[0045] Figure 2 This is the UV-Vis spectrum of the all-silicon molecular sieve (without metal element M nanoparticles).
[0046] Figure 3 This is a peak analysis diagram of the UV-Vis spectrum of the product prepared in Example 1.
[0047] Figure 4 The XRD spectrum of the product prepared in Example 1 is shown.
[0048] Figure 5 This is a SEM photograph of the product prepared in Example 1. DETAILED DESCRIPTION
[0049] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0050] The first aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material, comprising an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve;
[0051] The composite catalytic material has the following UV-Vis characteristics:
[0052] In the peak separation results of the wavelength of 450nm to 740nm in the UV-Vis spectrum of the composite catalytic material, the peak area of the spectrum peak in the wavelength range of 650 to 670nm is recorded as A 1 The total peak area within the wavelength range of 450nm to 740nm in the UV-Vis spectrum of the composite catalytic material is recorded as A 2 ,
[0053] A is defined as follows: 0 Any value between 0.4 and 0.6;
[0054] A 0 =A 1 / A 2 Formula (1).
[0055] The molecular sieve of the composite catalytic material has a large specific surface area, pore volume and macromolecular substrate reaction activity; and the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore molecular sieve; the A 0 When the molecular weight of the composite catalyst is any value between 0.45 and 0.6, the composite catalyst material has a high catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0056] In the present disclosure, the peak separation of wavelengths of 450 nm to 740 nm in the UV-Vis spectrum may be performed using conventional peak separation methods and software in the art.
[0057] The inventors of the present disclosure surprisingly found in a large number of experimental studies that when a metal precursor, a polyhydroxy auxiliary agent and a silanization agent are introduced into the molecular sieve synthesis process, the reaction mixture is subjected to hydrothermal crystallization, washing and calcination, and the obtained composite catalytic material including all-silicon molecular sieve and metal M oxide nanoparticles not only has a large specific surface area and pore volume performance, but also the metal oxide nanoparticles have uniform particle size and are evenly dispersed in the molecular sieve crystal (for example, in the molecular sieve mesopores), and may also exist on the surface of the molecular sieve pores; and the inventors also found that the UV-Vis spectrum (such as 1.4 nm) of the all-silicon molecular sieve without metal element M nanoparticles is different from that of the all-silicon molecular sieve. Figure 2 Compared with the above, after adding metal element M nanoparticles, the UV-Vis spectrum (as shown in Figure 1 As shown in FIG. 1 , a new peak appears near the wavelength range of 650 to 670 nm. The inventors have found through further research that the composite catalytic material has a peak in the range of 450 to 740 nm in the UV-Vis spectrum (as shown in FIG. Figure 3 The peak area of the spectrum peak in the wavelength range of 650 to 670 nm (A 1 ) and the total peak area (A 2 ) is related to the overall catalytic activity of the composite catalytic material, especially when A 0 (A 0 =A 1 / A 2 ) satisfies the range of 0.4 to 0.6, the composite catalytic material has good catalytic activity in the co-oxidation reaction of macromolecular aldehydes / olefins. For example, when used in the co-oxidation reaction of cyclooctene and isobutyraldehyde, a higher cyclooctene conversion rate and epoxycyclooctene selectivity can be obtained.
[0058] In a preferred embodiment, the A 0 The value of is any value between 0.45 and 0.6. 0 Within this range, the catalytic activity is higher, and the cyclooctene conversion rate and epoxycyclooctene selectivity are higher.
[0059] In one embodiment, the all-silicon molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve.
[0060] In one embodiment, the metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.
[0061] In one embodiment, the composite catalytic material includes silicon element, metal element M and oxygen element, and the molar ratio of the metal element M to the silicon element is (0.001-0.2):1, preferably (0.001-0.18):1.
[0062] In one embodiment, the metal element M in the composite catalytic material exists in the form of metal nanoparticles, the average particle size of the metal nanoparticles is 0.5 to 8 nm, and the BET specific surface area is 400 to 800 m 2 / g, the total pore volume is 0.3-0.65 mL / g, the micropore volume is 0.1-0.19 mL / g, and the mesopore volume is 0.2-0.46 mL / g. The composite catalytic material disclosed in the present invention also has a multi-level pore structure, which is conducive to catalyzing large-sized reaction substrates.
[0063] The second aspect of the present disclosure provides a method for preparing a composite catalytic material of metal nanoparticles and molecular sieves, comprising the following steps:
[0064] S1, mixing a template, a silicon source, water, a metal M precursor, a polyhydroxy auxiliary and a silanization agent to obtain a reaction mixture; wherein the polyhydroxy auxiliary is a compound containing at least two hydroxyl groups; and the silanization agent contains at least one coordination group capable of complexing with the metal element M;
[0065] S2. performing hydrothermal crystallization and calcination on the reaction mixture.
[0066] The present invention discloses introducing metal precursors, polyhydroxy additives and silanization agents during the hydrothermal crystallization synthesis of molecular sieves, which can simultaneously achieve the effects of highly dispersing metal oxide nanoparticles in the molecular sieve crystals and expanding the pores of the molecular sieve support layer, thereby preparing a multi-level porous molecular sieve composite catalytic material with highly dispersed metal oxide nanoparticles.
[0067] In the present disclosure, on the one hand, the metal ions in the reaction mixture are complexed with the polyhydroxy auxiliary agent to achieve the effect of dispersing and stabilizing the metal; at the same time, at least one coordination group of the silanization agent can also be complexed with the metal ions to achieve the effect of fixing and dispersing the metal, so that the metal oxide nanoparticles in the molecular sieve pores obtained after hydrothermal crystallization and calcination have high dispersion; on the other hand, the alkyl chain of the silanization agent also ensures the realization of the molecular sieve support layer expansion effect of the synthesized composite catalyst material. Thus, a multi-level porous all-silicon molecular sieve composite catalyst material with highly dispersed metal nanoparticles is finally prepared.
[0068] In one embodiment, in step S1, SiO 2The molar ratio of silicon source: template: water: metal M element: silanization agent is 1: (0.005-1): (10-80): (0.001-0.2): (0.025-0.4), preferably 1: (0.005-1): (10-80): (0.001-0.18): (0.025-0.3); the molar ratio of polyhydroxy auxiliary agent to metal element M is (0.2-2): 1, preferably (0.5-2): 1. Specifically, the water used in step S1 can be the water commonly used in the synthesis of molecular sieves, and in order to avoid the introduction of heteroatoms, it is preferably deionized water.
[0069] In a preferred embodiment, step S1 comprises:
[0070] a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution;
[0071] b. Adding a polyhydroxy auxiliary agent to an aqueous solution of a metal M precursor, and mixing the mixture to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material;
[0072] c. Adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture; preferably, the mixing conditions in step c include: stirring at 20 to 80° C. for 0.5 to 2 hours.
[0073] In one embodiment, in step S1, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black; the general formula of the organic silicone grease is the structure shown in the following formula (A):
[0074]
[0075] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight chain alkyl group having 1 to 4 carbon atoms or a branched chain alkyl group having 3 to 4 carbon atoms. a , R b , R c , R d Each is independently methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl. a , R b , R c, R d Each is independently methyl or ethyl.
[0076] In a preferred embodiment, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0077] In one embodiment, in step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;
[0078] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.
[0079] Preferably, the hydrolysis-alcohol removal treatment is performed so that the mass content of alcohol produced by hydrolysis of the obtained organic silicone grease in the hydrolysis solution of silicon is less than 10 ppm.
[0080] According to the present disclosure, in step S1, the template agent is an organic base, preferably at least one selected from quaternary ammonium base, aliphatic amine and aliphatic alcohol amine. The quaternary ammonium base can be an organic quaternary ammonium base; the aliphatic amine can be NH 3 A compound formed by replacing at least one hydrogen in the aliphatic hydrocarbon group (such as an alkyl group); the aliphatic alcohol amine can be various NH 3 A compound formed by replacing at least one hydrogen in a moiety with a hydroxyl-containing aliphatic group (such as an alkyl group).
[0081] Further preferably, the template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B):
[0082] R 1 , R 2 , R 3 and R 4 are independently selected from an alkyl group having 1 to 4 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms, more preferably R 1 , R 2 , R 3 and R 4 Each of the following is selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
[0083] The template agent is preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide (including various isomers of tetrapropylammonium hydroxide, such as tetra-n-propylammonium hydroxide and tetraisopropylammonium hydroxide) and tetrabutylammonium hydroxide (including various isomers of tetrabutylammonium hydroxide, such as tetra-n-butylammonium hydroxide and tetraisobutylammonium hydroxide).
[0084] In a preferred embodiment, the molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0085] In another preferred embodiment, the molecular sieve of the composite catalyst material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0086] In another preferred embodiment, the molecular sieve of the composite catalyst material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide. The present disclosure can prepare molecular sieves of different structures by selecting different template agents.
[0087] According to the present disclosure, the optional range of types of the metal precursor is relatively wide, and any substance containing the metal (such as a compound containing a metal element and / or a metal single substance) can achieve the purpose of the present disclosure.
[0088] In one embodiment, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the organic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;
[0089] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0090] Preferably, the metal M precursor is an aqueous solution of a metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0091] In one embodiment, in step S1, the general formula of the silanization agent is R 5 Si(R 6 )(R 7)R 8 , where R 5 , R 6 , R 7 , R 8 are independently halogen, alkyl, alkoxy, aromatic, mercapto or amine, and R 5 , R 6 , R 7 , R 8 At least one of the groups is an alkyl group, an alkoxy group, an aromatic group, a thiol group or an amine group; the alkyl group, the alkoxy group, the thiol group and the amine group each independently have 1 to 18 carbon atoms, preferably 1 to 12 carbon atoms, and the aromatic group has 6 to 18 carbon atoms, preferably 6 to 12 carbon atoms;
[0092] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0093] In one embodiment, in step S1, the polyhydroxy auxiliary agent is selected from one or more of polyols and sugar substances;
[0094] Preferably, the polyol comprises one or more of ethylene glycol, glycerol, pentaerythritol, 1,2-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, neopentyl glycol, diethylene glycol and polyether polyol; wherein the polyether polyol comprises one or more of propylene glycol polyether, trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol; the weight average molecular weight of the propylene glycol polyether is 800-2000, and the weight average molecular weight of the trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol is independently 400-4000;
[0095] The sugar substances include one or more of glucose, sucrose, fructose, starch and cellulose.
[0096] In one embodiment, in step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C.
[0097] In one embodiment, in step S2, the conditions of the calcination treatment include: a calcination temperature of 400-900° C., and a calcination time of 1-16 hours; preferably, the calcination temperature is 400-800° C., and the calcination time is 2-8 hours.
[0098] A third aspect of the present disclosure provides a metal nanoparticle and molecular sieve composite catalytic material prepared according to the method described in the second aspect of the present disclosure.
[0099] The fourth aspect of the present disclosure provides the use of the metal nanoparticles and molecular sieve composite catalytic material described in the first aspect or the third aspect of the present disclosure in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins; preferably, the use in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0100] In a specific embodiment, the reaction conditions in the use of catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde include: the molar ratio of isobutyraldehyde to cyclooctene is 2 to 8:1, the weight ratio of the metal nanoparticles to the molecular sieve composite catalytic material is 1 to 20 weight % based on the total weight of isobutyraldehyde and cyclooctene; 0.1 to 2 MPa, the reaction temperature is 20 to 120° C., and the reaction time is 2 to 48 hours. Optionally, the reaction is carried out in a slurry bed reactor.
[0101] When the composite catalytic material is used to catalyze the co-oxidation reaction of cyclooctene and isobutyraldehyde, the conversion rate of cyclooctene is not less than 75 mol %, the selectivity of the target product epoxy cyclooctene is not less than 85 mol %, and the conversion rate of isobutyraldehyde is not less than 98 mol %.
[0102] The present disclosure will be further described below using embodiments.
[0103] In the present disclosure, the solid ultraviolet-visible diffuse reflectance spectrum (UV-vis) of the sample was measured on a SHIMADZU UV-3100 ultraviolet-visible spectrometer in the test range of 400 to 4000 cm -1 .
[0104] The X-ray diffraction (XRD) crystal phase diagram of the sample was determined on a Siemens D5005 X-ray diffractometer, the radiation source was Kα (Cu), and the test range 2θ was 0.5° to 70°.
[0105] The SEM images of the samples were obtained on a Hitachi S4800 high-resolution cold field emission scanning electron microscope.
[0106] The TEM images of the samples were obtained on a FEI Tecnai G2F20S-TWIN transmission electron microscope. The average particle size of the metal oxide nanoparticles was obtained based on TEM electron microscope testing.
[0107] The total specific surface area and total pore volume of the sample were measured on a Micromeritics ASAP245 static nitrogen adsorption instrument according to the ASTM D4222-98 standard method. The adsorption isotherm and desorption isotherm of low-temperature nitrogen adsorption of the sample were measured according to the ASTM D4222-98 standard method.
[0108] Example 1
[0109] (1) 1.6 g of 25.05 wt% tetrapropylammonium hydroxide (TPAOH, 0.002 mol) aqueous solution, 20.8 g of tetraethyl silicate (0.1 mol) and 52.8 g (3 mol) of water were added to a 500 mL beaker in sequence, and the mixture was placed on a magnetic stirrer with heating and stirring functions to mix evenly, and stirred at 50° C. for 2 hours, and the evaporated water was replenished regularly to obtain a colorless and transparent silicon hydrolysis solution;
[0110] (2) 0.03 g of cobalt nitrate hexahydrate (0.1 mmol) and 0.18 g (0.01 mol) of water were stirred evenly, and then 0.05 mmol of ethylene glycol was added to mix the aqueous solution of cobalt with the hydrolyzed solution of silicon obtained in step (1);
[0111] (3) Add 0.64 g of N-phenyl-3-aminopropyltrimethoxysilane (PHAPTMS, 0.0025 mol) to the mixture of step (2) and stir for 0.5 hour;
[0112] (4) The mixture obtained in step (3) is transferred to a stainless steel closed reactor and crystallized at a constant temperature of 175° C. for 24 hours to obtain a sample. The obtained sample is filtered, washed, dried at 110° C. for 6 hours, and then calcined in a muffle furnace at 550° C. for 6 hours to obtain a metal nanoparticle and molecular sieve composite catalytic material product, which is recorded as C1.
[0113] The BET specific surface area, total pore volume, micropore volume, mesopore volume and average particle size of the metal nanoparticles contained in C1 are listed in Table 2.
[0114] UV-Vis image of C1 Figure 1 The peak separation results are shown in Figure 3 As shown in Figure 1, three peaks are separated in the range of 450-740 nm: the peak at 520 nm represents the species inside the cobalt oxide nanoparticles, the peak at 590 nm represents the species at the interface between the cobalt oxide nanoparticles and the silicon skeleton, and the peak at 660 nm represents the species on the surface of the cobalt oxide nanoparticles (active centers). The XRD spectrum of product C1 is shown in Figure 1. Figure 4 As shown in Figure 2, XRD analysis shows that it has an MFI structure. The SEM image of the product is shown in Figure 2. Figure 5As shown, it can be seen that the product prepared in this example has a regular shape and uniform size.
[0115] Comparative Example 1
[0116] This comparative example was prepared according to the method of Example 1, except that no silanization agent was added. The proportions, synthesis conditions and results are listed in Table 1. Other conditions and operations refer to Example 1. The prepared product is recorded as sample D-1.
[0117] Comparative Example 2
[0118] This comparative example was prepared according to patent CN 111847471 A.
[0119] Under stirring conditions, ethyl orthosilicate, tetrapropylammonium hydroxide, cobalt nitrate and deionized water are mixed to obtain a molar ratio of SiO 2 :Structure directing agent:Co:H 2 O=1:0.2:0.001:30 first mixture; then SiO 2 :Silane reagent = 1:0.025 molar ratio, PHAPTMS is added to the above first mixture, after stirring evenly, the obtained second mixture is transferred to a pressure-resistant stainless steel reactor; under stirring conditions, it is heated to 170°C and crystallized under autogenous pressure for 8 hours. After the stainless steel pressure-resistant reactor cools to room temperature, the crystallized product is recovered, dried at 110°C for 6 hours, and then calcined at 550°C for 4 hours to obtain a multi-level porous molecular sieve encapsulating cobalt. The prepared product is recorded as sample D-2.
[0120] Comparative Example 3
[0121] This comparative example was prepared according to the method of Ning Wang et al. (JACS, 2016, Vol. 138, pp. 7484-7487).
[0122] Deionized water was first mixed with 13 g of TPAOH solution and stirred continuously for 10 minutes, and then 8.32 g of ethyl orthosilicate (0.04 mol) was added. After continuous stirring for 6 hours, the mixture became clear after complete hydrolysis. 0.052 g of cobalt nitrate hexahydrate (0.18 mmol, the molar ratio of metal cobalt to silicon source was 0.0045) was dissolved in a mixture of 0.3 mL of ethylenediamine and 3 mL of water to prepare [Pd(NH 2 CH 2 CH 2 NH 2 ) 2 ]Cl 2The obtained solution was then added dropwise to the above mixture and stirred for 30 min without precipitation. The reaction mixture was transferred to a 100 mL stainless steel autoclave with a polytetrafluoroethylene liner and subjected to static crystallization at 170 ° C for 4 days in a conventional oven. The obtained solid product was centrifuged, washed with water and ethanol several times, dried in an oven at 80 ° C overnight, calcined in an air atmosphere at 550 ° C for 8 hours, and finally reduced with hydrogen to obtain the product. The prepared product was recorded as sample D-3.
[0123] Embodiment 2 to Embodiment 9
[0124] The corresponding products C2-C9 were prepared according to the method of Example 1, and their proportions, synthesis conditions and results are listed in Table 1. Other conditions and operations refer to Example 1.
[0125] Example 10
[0126] The cobalt-containing multi-level porous β molecular sieve was prepared by referring to the method of Example 1, changing the ratio and template agent. The template agent used was tetraethylammonium hydroxide (TEAOH). The ratio, synthesis conditions and results are shown in Table 1. The product is recorded as C10.
[0127] Embodiment 11
[0128] The cobalt-containing multi-level porous MEL molecular sieve was prepared by referring to the method of Example 1, changing the ratio and template agent. The template agent used was tetrabutylammonium hydroxide (TBAOH). The ratio, synthesis conditions and results are shown in Table 1. The product is recorded as C11.
[0129] Example 12
[0130] The corresponding product was prepared according to the method of Example 1, and its ratio, synthesis conditions and results are listed in Table 1. Other conditions and operations refer to Example 1, and the product is recorded as C12.
[0131] The hydrothermal crystallization temperature is 120°C and the hydrothermal crystallization time is 6 days; the calcination temperature is 870°C and the calcination time is 9 hours.
[0132] The BET specific surface area, total pore volume, micropore volume, mesopore volume and average particle size of metal nanoparticles contained in the composite catalytic material of the products obtained in the above examples and comparative examples are listed in Table 2 below.
[0133] Table 1
[0134]
[0135]
[0136] In Table 1, the cobalt nitrate used is all cobalt nitrate hexahydrate; TPAOH is tetrapropylammonium hydroxide, TPABr is tetrapropylammonium bromide, TBAOH is tetrabutylammonium hydroxide, TEAOH is tetraethylammonium hydroxide; PHAPTMS is N-phenyl-3-aminopropyltrimethoxysilane, APTES is 3-aminopropyltriethoxysilane, and KH792 is a silane coupling agent kh792 (bisamino functional group silane, N-aminoethyl-γ-aminopropyltrimethoxysilane). The reagents used in the present disclosure can be obtained through conventional purchasing channels.
[0137] Table 2
[0138]
[0139]
[0140] Among them, pores with a diameter less than 2nm are micropores, and pores with a diameter between 2 and 50nm are mesopores.
[0141] According to Table 2, compared with D-1 prepared in Comparative Example 1 (without adding silanization agent) and D-3 prepared in Comparative Example 3 (without adding silanization agent), C1~C12 prepared in Examples 1~12 of the present disclosure by adding silanization agent during the preparation process have higher mesopore volume, indicating that the method provided in the present disclosure can effectively expand the pores of the molecular sieve.
[0142] Compared with D-2 prepared in Comparative Example 2 (without adding a polyhydroxy auxiliary agent), C1-C12 prepared in the present disclosure have a smaller average particle size of metal nanoparticles, indicating that the C1-C12 nanoparticles have a lower degree of aggregation and a higher degree of dispersion.
[0143] Test Case
[0144] This test example illustrates the reaction effects of the samples prepared in the examples and comparative examples provided in the present disclosure for the co-oxidation reaction of cyclooctene and isobutyraldehyde.
[0145] The reagents used in this test example are all commercially available chemically pure reagents, and the concentrations of various substances after the reaction are quantitatively analyzed using gas chromatography. The gas chromatograph used is a 6890 gas chromatograph produced by Agilent; the analytical chromatographic column used is an HP-5 column.
[0146] The conversion rate of cyclooctene, the conversion rate of isobutyraldehyde and the selectivity of cyclooctene oxide in the examples are calculated according to the following formulas (2)-(4):
[0147]
[0148]
[0149]
[0150] The samples prepared in the comparative example and the example were taken respectively, and were uniformly stirred and mixed in a slurry bed according to a molar ratio of isobutyraldehyde:cyclooctene=3:1. The slurry bed closed system was connected to a normal pressure pure oxygen balloon as an oxygen source, the oxygen pressure was 0.1MPa, the amount of cyclooctene was 1mmol, the amount of catalyst was 50mg, and the amount of solvent acetonitrile was 2.5mL. The reaction was stable at 25°C for 6 hours, and the samples were taken for analysis. The results are shown in Table 3.
[0151] Table 3
[0152]
[0153] According to the data in Table 3, compared with D-1 to D-3 prepared in Comparative Examples 1 to 3, the A 0 In the range of 0.4 to 0.6, the catalyst has higher catalytic activity in the co-oxidation reaction of cyclooctene and isobutyraldehyde, and the cyclooctene conversion rate and epoxycyclooctene selectivity are higher.
[0154] Comparing C1~C11 with C12, we can see that the A of C1~C11 0 When the value is in the range of 0.45 to 0.6, the catalytic effect of C1 to C11 is better, and the cyclooctene conversion rate and epoxycyclooctene selectivity are higher.
[0155] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0156] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0157] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A metal nanoparticle and molecular sieve composite catalytic material, characterized in that: It comprises an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve; the metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; The composite catalytic material has the following UV-Vis characteristics: In the peak separation results of the wavelength of 450-740nm in the UV-Vis spectrum of the composite catalytic material, the peak area of the spectrum peak in the wavelength range of 650-670nm is recorded as A1, and the total peak area in the wavelength range of 450-740nm in the UV-Vis spectrum of the composite catalytic material is recorded as A2. A0 defined by the following formula (1) is any value between 0.4 and 0.6; A0=A1 / A2 (1); The metal nanoparticle and molecular sieve composite catalytic material is prepared by a method comprising the following steps: S1, mixing a template, a silicon source, water, a metal M precursor, a polyhydroxy auxiliary and a silanization agent to obtain a reaction mixture; wherein the polyhydroxy auxiliary is a compound containing at least two hydroxyl groups; the silanization agent contains at least one ligand group that can complex with the metal element M; the polyhydroxy auxiliary is selected from one or more of polyols and sugar substances; S2. performing hydrothermal crystallization and calcination on the reaction mixture.
2. The composite catalytic material according to claim 1, characterized in that: The value of A0 is any value between 0.45 and 0.
6.
3. The composite catalytic material according to claim 1, characterized in that: The all-silicon molecular sieve in the composite catalytic material is at least one of an MFI structure molecular sieve, a MEL structure molecular sieve, a BEA structure molecular sieve, an MWW structure molecular sieve, a two-dimensional hexagonal structure molecular sieve, a MOR structure molecular sieve and a TUN structure molecular sieve.
4. The composite catalytic material according to claim 3, characterized in that: The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the group consisting of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve.
5. The composite catalytic material according to claim 4, characterized in that: The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the MFI structure molecular sieve, the MEL structure molecular sieve and the BEA structure molecular sieve.
6. The composite catalytic material according to claim 1, characterized in that: In the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.2):
1.
7. The composite catalytic material according to claim 6, characterized in that: In the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.18):
1.
8. The composite catalytic material according to claim 1, characterized in that: The BET specific surface area of the composite catalytic material is 400-800 m 2 / g, the total pore volume is 0.3~0.65mL / g, the micropore volume is 0.1~0.19mL / g, the mesopore volume is 0.2~0.46mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5~8nm.
9. The composite catalytic material according to claim 1, characterized in that: In step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent calculated as SiO2 is 1: (0.005~1): (10~80): (0.001~0.2): (0.025~0.4); the molar ratio of polyhydroxy auxiliary agent to metal element M is (0.2~2):
1.
10. The composite catalytic material according to claim 9, characterized in that: In step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent calculated as SiO2 is 1: (0.005~1): (10~80): (0.001~0.18): (0.025~0.3); the molar ratio of polyhydroxy auxiliary agent to metal element M is (0.5~2):
1.
11. The composite catalytic material according to claim 1, characterized in that: Step S1 includes: a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution; b. Adding a polyhydroxy auxiliary agent to an aqueous solution of a metal M precursor, and mixing the mixture to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material; c. Adding a silanization agent into the second mixed material and mixing them to obtain the reaction mixture.
12. The composite catalytic material according to claim 11, characterized in that: The mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
13. The composite catalytic material according to claim 1, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol.
14. The composite catalytic material according to claim 13, characterized in that: The silicon source is selected from at least one of organic silicone grease, solid silica gel and white carbon black.
15. The composite catalytic material according to claim 14, characterized in that: The silicon source is organic silicone grease, and the general formula of the organic silicone grease is the structure shown in the following formula (A): (A); Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, and the alkyl group is a branched or straight chain alkyl group.
16. The composite catalytic material according to claim 15, characterized in that: In formula (A), R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms.
17. The composite catalytic material according to claim 16, characterized in that: In formula (A), R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
18. The composite catalytic material according to claim 17, characterized in that: In formula (A), the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
19. The composite catalytic material according to claim 11, characterized in that: In step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain a hydrolyzed solution of the silicon; The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0-95° C. for 2-10 hours.
20. The composite catalytic material according to claim 19, characterized in that The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 50-95° C. for 2-8 hours.
21. The composite catalytic material according to claim 1, characterized in that: In step S1, the template agent is an organic base.
22. The composite catalytic material according to claim 21, characterized in that The template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.
23. The composite catalytic material according to claim 22, characterized in that: The template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B): (B); R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms.
24. The composite catalytic material according to claim 23, characterized in that In formula (B), R1, R2, R3 and R4 are independently selected from a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 4 carbon atoms.
25. The composite catalytic material according to claim 24, characterized in that: In formula (B), R1, R2, R3 and R4 are each selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
26. The composite catalytic material according to claim 1, characterized in that The molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or The molecular sieve of the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or The molecular sieve of the composite catalytic material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
27. The composite catalytic material according to claim 1, characterized in that In step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M.
28. The composite catalytic material according to claim 27, characterized in that The metal M precursor is a water-soluble inorganic salt of metal M.
29. The composite catalytic material according to claim 11, characterized in that: The molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
30. The composite catalytic material according to claim 1, characterized in that In step S1, the polyol of the polyhydroxy auxiliary agent includes one or more of ethylene glycol, glycerol, pentaerythritol, 1,2-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, neopentyl glycol, diethylene glycol and polyether polyol; wherein the polyether polyol includes one or more of propylene glycol polyether, trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol; the weight average molecular weight of the propylene glycol polyether is 800-2000, and the weight average molecular weight of the trimethylolpropane polyether, polyoxypropylene glycol, polyoxypropylene triol and polytetrahydrofuran diol is each independently 400-4000; The sugar substances include one or more of glucose, sucrose, fructose, starch and cellulose.
31. The composite catalytic material according to claim 1, characterized in that In step S1, the general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the alkyl group, the alkoxy group, the thiol group, and the amine group each independently have 1 to 18 carbon atoms, and the aromatic group has 6 to 18 carbon atoms.
32. The composite catalytic material according to claim 31, characterized in that The silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
33. The composite catalytic material according to claim 32, characterized in that The silanization agent is selected from at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
34. The composite catalytic material according to claim 1, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; The conditions of the calcination treatment include: a calcination temperature of 400-900° C. and a calcination time of 1-16 hours.
35. The composite catalytic material according to claim 34, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.; The conditions of the calcination treatment include: a calcination temperature of 400-800° C. and a calcination time of 2-8 hours.
36. Use of the metal nanoparticle and molecular sieve composite catalytic material according to any one of claims 1 to 35 in catalyzing the co-oxidation reaction of macromolecular aldehydes / olefins.
37. The use according to claim 36, characterized in that The use includes use of the metal nanoparticles and molecular sieve composite catalytic material in catalyzing the co-oxidation reaction of cyclooctene and isobutyraldehyde.