A high entropy alloy aerogel for fuel cell, preparation method thereof and fuel cell
By stirring the metal salt solution and stabilizer in an inert gas atmosphere and adding reducing agents, a high-entropy alloy aerogel was prepared, which solved the problem of difficulty in mixing multiple metal elements and achieved efficient preparation of the catalytic layer of the high-temperature fuel cell. Improved electrical performance and stability.
Patent Information
- Application Number
- CN202310088895.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-02-09
AI Technical Summary
The prior art is difficult to mix multiple metal elements with large differences in physical and chemical properties, which limits the development of high-entropy alloys, especially in the preparation of aerogel-like high-entropy alloys, traditional methods such as arc smelting and powders. The metallurgical industry cannot achieve it.
In an inert gas atmosphere, the metal salt solution is stirred evenly with the stabilizer, and the reducing agent is added to react. After washing and drying, a high-entropy alloy aerogel with a large specific surface area and excellent electrical properties is prepared for high-temperature protons. The catalytic layer of the exchange membrane fuel cell.
The preparation of high-entropy alloy aerogel has a large specific surface area, excellent electrical properties and self-supporting ability, avoids carrier corrosion, improves the resistance to free radicals and phosphoric acid poisoning under high temperature conditions, and simplifies the The preparation process reduces costs and improves production efficiency.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a high entropy alloy aerogel for fuel cells, a preparation method thereof and a fuel cell. Background Art
[0002] Compared with traditional energy conversion technologies such as internal combustion engines, fuel cells are highly efficient energy conversion devices that convert chemical energy in fuel into electrical energy. The reaction process is not limited by the Carnot cycle and has higher energy conversion efficiency and lower greenhouse gas emissions. Among many fuel cells, proton exchange membrane fuel cells have attracted much attention due to their cleanliness, high efficiency, zero pollution, low operating temperature, and rapid startup. As a key component of proton exchange membrane fuel cells, proton exchange membrane (PEM) is mainly responsible for transmitting protons and blocking fuel penetration. Its performance directly determines the service life and efficiency of the fuel cell.
[0003] The operating temperature of high-temperature proton membrane fuel cells does not need to rely on the presence of water during operation, which can simplify the hydrothermal management of the system, and the increase in ambient temperature can greatly improve the reaction kinetics. However, during long-term operation, phosphoric acid penetrates into the catalytic layer and poisons the Pt / C catalyst, reducing the catalytic activity; secondly, the carbon carrier in the traditional Pt / C catalyst is easily corroded in high-temperature environments, further reducing the catalytic performance.
[0004] High entropy alloys are new functional materials composed of five or more metal materials. In the design process, they are formulated according to the characteristics of multiple main elements, and the synergy of multiple mechanisms is brought into play, making it possible to obtain an adsorption energy curve close to continuous distribution. The optimal adsorption strength is obtained through multi-element alloying, thereby maximizing the activity and improving the resistance to phosphoric acid poisoning, showing great application potential in the field of high-temperature proton exchange membrane fuel cells.
[0005] However, how to make full use of the active sites of high entropy alloy catalysts, improve electrocatalytic activity and stability is a key problem to promote the development of high entropy alloys in the field of catalysis. Aerogels have the characteristics of low density, high porosity and large internal surface area, and extend the characteristics of nanomaterials to the macroscopic scale through self-assembly. High entropy alloys are prepared into aerogels, whose large internal specific surface area provides a large number of catalytic active sites, high porosity is conducive to oxygen transmission and exposure of active sites, and ductile surface deformation structure gives it high electrocatalytic stability. In addition, traditional carbon support materials are abandoned to avoid carrier corrosion and improve stability under high temperature proton membrane fuel cell conditions.
[0006] However, conventional preparation methods make it difficult to mix multiple metal elements with greatly different physical and chemical properties, which limits the development of high entropy alloys. Traditional arc melting and powder metallurgy industries cannot produce aerogel-like high entropy alloys. Summary of the invention
[0007] Based on this, the embodiment of the present invention provides a high entropy alloy aerogel for fuel cells, a preparation method thereof and a fuel cell, aiming to solve the problem that multiple elements in existing high entropy alloys are difficult to mix. The present application can mix multiple metal elements with large differences in physical and chemical properties to prepare a high entropy alloy aerogel for high-temperature proton exchange membrane fuel cells.
[0008] To achieve the above objectives, on the one hand, an embodiment of the present invention provides a method for preparing a high entropy alloy aerogel for a fuel cell, comprising the following steps:
[0009] S01. In an inert gas atmosphere, add a metal salt solution to a stabilizer and stir evenly to obtain a metal precursor mixed solution; the molar ratio of the metal salt in the metal salt solution to the stabilizer is 1:(3-5);
[0010] S02, adding a reducing agent to the metal precursor mixed solution of step S01, stirring and reacting at 50° C. to 80° C. for 1 h to 6 h, and then aging for 12 h to 24 h to obtain a metal nanoparticle sol;
[0011] S03, washing and drying the metal nanoparticle sol in step S02 to obtain a high entropy alloy aerogel for a fuel cell.
[0012] As a preferred embodiment, in step S01,
[0013] The inert gas is nitrogen, argon or helium.
[0014] The concentration of the metal salt solution is 1 mmol / L to 5 mmol / L.
[0015] The metal salt solution includes at least five metal salts. Taking the sum of the molar numbers of the five metal salts as 100%, the molar proportions of metal ions in the five metal salts are all 15% to 25%.
[0016] The metal salt solution is a mixture of at least five of a platinum salt solution, a palladium salt solution, a gold salt solution, a nickel salt solution, a copper salt solution and a cobalt salt solution.
[0017] The platinum salt solution is preferably one or a mixed solution of at least two of H2PtCl6·6H2O, Na2PtCl6 and K2PtCl6.
[0018] The palladium salt solution is preferably one of H2PdCl4, Na2PdCl4 and K2PdCl4 or a mixture of at least two of them.
[0019] The gold salt solution is preferably one of HAuCl4·3H2O, NaAuCl4 and KAuCl4, or a mixture of at least two of them.
[0020] The nickel salt solution is preferably a mixture of one or both of Ni(NO3)2 and NiCl2.
[0021] The copper salt solution is preferably a mixture of one or both of Cu(NO3)2 and CuCl2.
[0022] The cobalt salt solution is preferably a mixture of one or both of Co(NO3)2 and CoCl2.
[0023] The stabilizer is one of citric acid, sodium citrate, polyvinyl pyrrolidone and cyclohexane or a mixture of at least two of them.
[0024] The stirring time is 30 min to 60 min, preferably 30 min.
[0025] As a preferred embodiment, in step S02,
[0026] The reducing agent is one or a mixture of at least two of NaHB4, ascorbic acid and sodium hypophosphite.
[0027] As a preferred embodiment, in step S03,
[0028] The washing is preferably performed with water; the number of washings is preferably 6 times.
[0029] The drying is preferably carried out by supercritical CO2 drying; the drying temperature is preferably 35°C, the drying pressure is preferably 7.5MPa, and the drying time is preferably 3h.
[0030] On the other hand, an embodiment of the present invention also provides a high entropy alloy aerogel for a fuel cell prepared by the above preparation method.
[0031] On the other hand, an embodiment of the present invention further provides a fuel cell, wherein the fuel cell includes a proton exchange membrane, and the high entropy alloy aerogel for the fuel cell is disposed on a side of the proton exchange membrane.
[0032] Preferably, the proton exchange membrane is a high-temperature proton exchange membrane.
[0033] The present application can effectively solve the problem that multiple elements in existing high entropy alloys are difficult to mix. The present application mixes multiple metal elements with large differences in physical and chemical properties to prepare high entropy alloy aerogels for high-temperature proton exchange membrane fuel cells. The high entropy alloy aerogel has a large specific surface area, excellent electrical properties and self-supporting ability, and can be directly used as a catalyst layer for high-temperature fuel cells to avoid the collapse of the catalyst layer structure due to carrier corrosion. The high entropy alloy aerogel for fuel cells in the present application can adjust the proportion of different metal elements according to actual needs, change the electronic structure of the alloy, and has a wide adjustable range, which can maximize the activity and improve the resistance of high entropy alloy aerogels for fuel cells under high temperature conditions. Free radicals and phosphoric acid poisoning resistance. The preparation method of the present application is simple, the preparation cost is low, the preparation time is short, the production efficiency is high, and it is easy to batch or large-scale production.
[0034] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments. DETAILED DESCRIPTION
[0035] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, top, bottom...), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0037] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0038] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.
[0039] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0040] At present, it is difficult to mix multiple metal elements with different physical and chemical properties in the existing conventional preparation methods, which limits the development of high entropy alloys. The traditional arc melting method and powder metallurgy industry cannot obtain aerogel-like high entropy alloys. Based on this, it is necessary to provide a high entropy alloy aerogel for fuel cells, a preparation method thereof and a fuel cell to solve the above technical problems.
[0041] To achieve the above objectives, on the one hand, an embodiment of the present invention provides a method for preparing a high entropy alloy aerogel for a fuel cell, comprising the following steps:
[0042] S01. In an inert gas atmosphere, add a metal salt solution to a stabilizer and stir evenly to obtain a metal precursor mixed solution; the molar ratio of the metal salt in the metal salt solution to the stabilizer is 1:(3-5);
[0043] S02, adding a reducing agent to the metal precursor mixed solution of step S01, stirring and reacting at 50° C. to 80° C. for 1 h to 6 h, and then aging for 12 h to 24 h to obtain a metal nanoparticle sol;
[0044] S03, washing and drying the metal nanoparticle sol in step S02 to obtain a high entropy alloy aerogel for a fuel cell.
[0045] As a preferred embodiment, in step S01,
[0046] The molar ratio of the metal salt in the metal salt solution to the stabilizer may be 1:3, 1:4 or 1:5, etc., preferably 1:3.
[0047] The inert gas is nitrogen, argon or helium, preferably nitrogen.
[0048] The concentration of the metal salt solution is 1mmol / L to 5mmol / L. For example, the concentration can be set to 1mmol / L, 2mmol / L, 3mmol / L, 4mmol / L or 5mmol / L, etc. according to actual needs, so that a variety of metal elements with large differences can be mixed, and the prepared high entropy alloy aerogel has a large specific surface area, excellent electrical properties and self-supporting ability. The metal salt solution includes at least five metal salts, and the sum of the molar numbers of the five metal salts is 100%, and the molar proportion of the metal ions in the five metal salts is 15% to 25% (such as 15%, 18%, 20%, 23%, or 25%, etc.). For example, in an embodiment of the present application, the molar ratio of the metal ions in the five metal salts is 1:1:1:1:1 (that is, the molar proportion is 20%). In this way, a variety of metal elements with large differences can be mixed, and the prepared high entropy alloy aerogel has a large specific surface area, excellent electrical properties and self-supporting ability.
[0049] The metal salt solution is a mixture of at least five of a platinum salt solution, a palladium salt solution, a gold salt solution, a nickel salt solution, a copper salt solution and a cobalt salt solution.
[0050] The platinum salt solution is preferably one or a mixed solution of at least two of H2PtCl6·6H2O, Na2PtCl6 and K2PtCl6, more preferably H2PtCl6·6H2O.
[0051] The palladium salt solution is preferably one of H2PdCl4, Na2PdCl4 and K2PdCl4 or a mixture of at least two of them, more preferably H2PdCl4.
[0052] The gold salt solution is preferably one of HAuCl4·3H2O, NaAuCl4 and KAuCl4 or a mixture of at least two of them, more preferably HAuCl4·3H2O.
[0053] The nickel salt solution is preferably Ni(NO3)2 and NiCl2 or a mixture of both, more preferably NiCl2.
[0054] The copper salt solution is preferably a mixture of one or both of Cu(NO3)2 and CuCl2, more preferably CuCl2.
[0055] The cobalt salt solution is preferably a mixture of one or both of Co(NO3)2 and CoCl2, more preferably CoCl2.
[0056] The stabilizer is one of citric acid, sodium citrate, polyvinyl pyrrolidone and cyclohexane or a mixture of at least two of them, preferably citric acid. This ensures that a variety of metal elements with large differences are mixed, and ensures that the prepared high entropy alloy aerogel has a large specific surface area, excellent electrical properties and self-supporting ability.
[0057] The stirring time is 30 min to 60 min, preferably 30 min. This ensures that a variety of metal elements with large differences are mixed, and ensures that the prepared high entropy alloy aerogel has a large specific surface area, excellent electrical properties and self-supporting ability.
[0058] As a preferred embodiment, in step S02,
[0059] The reducing agent is one or a mixture of at least two of NaHB4, ascorbic acid and sodium hypophosphite, preferably NaHB4. This ensures that a variety of metal elements with large differences are mixed, and ensures that the prepared high entropy alloy aerogel has a large specific surface area, excellent electrical properties and self-supporting ability. The amount of the reducing agent is generally excessive, that is, an excessive amount of the reducing agent is used for the reaction.
[0060] As a preferred embodiment, in step S03,
[0061] The washing is preferably performed with water; the number of washings is preferably 6 times.
[0062] The drying is preferably carried out by supercritical CO2 drying; the drying temperature is preferably 35°C, the drying pressure is preferably 7.5 MPa, and the drying time is preferably 3 hours. In this way, by replacing the solvent of the metal nanoparticle sol with liquid CO2, a high entropy alloy aerogel for fuel cells is obtained.
[0063] On the other hand, the embodiment of the present invention also provides a high entropy alloy aerogel for fuel cells prepared by the above preparation method. The high entropy alloy aerogel for fuel cells can be directly used as a catalyst layer of a high-temperature fuel cell to avoid the collapse of the catalyst layer structure due to carrier corrosion.
[0064] On the other hand, an embodiment of the present invention further provides a fuel cell, wherein the fuel cell includes a proton exchange membrane, and the high entropy alloy aerogel for the fuel cell is disposed on a side of the proton exchange membrane.
[0065] Preferably, the proton exchange membrane is a high temperature (generally the temperature is higher than 100° C.) proton exchange membrane.
[0066] In one of the embodiments, in the fuel cell structure, the fuel cell prepared in the embodiment of the present application uses high entropy alloy aerogel to replace the catalyst layer and the gas diffusion layer and arranges them on both sides of the proton exchange membrane, and other structural components of the fuel cell use conventional components and are arranged in a conventional manner.
[0067] In another embodiment, in the fuel cell structure, the fuel cell prepared in the embodiment of the present application uses a high entropy alloy aerogel to replace the catalyst layer and arranges it on both sides of the proton exchange membrane, and other structural components of the fuel cell use conventional components and are arranged in a conventional manner.
[0068] The present application can effectively solve the problem that multiple elements in existing high entropy alloys are difficult to mix. The present application mixes multiple metal elements with large differences in physical and chemical properties to prepare high entropy alloy aerogels for high-temperature proton exchange membrane fuel cells. The high entropy alloy aerogel has a large specific surface area, excellent electrical properties and self-supporting ability, and can be directly used as a catalyst layer for high-temperature fuel cells to avoid the collapse of the catalyst layer structure due to carrier corrosion. The high entropy alloy aerogel for fuel cells in the present application can adjust the proportion of different metal elements according to actual needs, change the electronic structure of the alloy, and has a wide adjustable range, which can maximize the activity and improve the resistance of high entropy alloy aerogels for fuel cells under high temperature conditions. Free radicals and phosphoric acid poisoning resistance. The preparation method of the present application is simple, the preparation cost is low, the preparation time is short, the production efficiency is high, and it is easy to batch or large-scale production.
[0069] Example 1
[0070] A method for preparing a high entropy alloy aerogel for a fuel cell comprises the following steps:
[0071] S01. In an inert gas atmosphere, add a metal salt solution to a stabilizer and stir evenly to obtain a metal precursor mixed solution; the molar ratio of the metal salt to the stabilizer in the metal salt solution is 1:3;
[0072] S02, adding a reducing agent (excessive amount) to the metal precursor mixed solution of step S01, stirring and reacting at 60° C. for 2 h, and then aging for 24 h to obtain a metal nanoparticle sol;
[0073] S03, washing and drying the metal nanoparticle sol in step S02 to obtain a high entropy alloy aerogel for a fuel cell.
[0074] In step S01,
[0075] The inert gas is nitrogen.
[0076] The concentration of the metal salt solution is 2 mmol / L.
[0077] The metal salt solution includes five metal salts, and the molar ratio of metal ions in the five metal salts is 1:1:1:1:1.
[0078] The metal salt solution is a mixture of a platinum salt solution, a palladium salt solution, a gold salt solution, a nickel salt solution and a copper salt solution.
[0079] The salt solution of platinum is H2PtCl6·6H2O. The salt solution of palladium is H2PdCl4. The salt solution of gold is HAuCl4·3H2O. The salt solution of nickel is NiCl2. The salt solution of copper is CuCl2.
[0080] The stabilizer is citric acid.
[0081] The stirring time is 30min.
[0082] In step S02,
[0083] The reducing agent is NaHB4.
[0084] In step S03,
[0085] The washing is performed with water; the number of washing times is 6 times.
[0086] The drying is carried out by supercritical CO2 drying; the drying temperature is 35°C, the drying pressure is 7.5MPa, and the drying time is 3h.
[0087] The prepared high entropy alloy aerogel (Pt-Pd-Au-Ni-Cu) for fuel cells has a particle size of 10nm to 50nm and a density of 0.10g / cm 3 , specific surface area 76.5m 2 / g, half-wave potential 0.89V, mass specific activity up to 0.31A / cm 2 @0.9V Pt / g , the oxygen reduction electron transfer number is 3.88, and the half-wave potential drops by 5mV after 10,000 cycles of 1V to 1.5V.
[0088] The fuel cell prepared in this embodiment uses high entropy alloy aerogel to replace the catalyst layer and the gas diffusion layer and arranges them on both sides of the proton exchange membrane to prepare a fuel cell, and the other structural components of the fuel cell are conventional components and can be arranged in a conventional manner. The prepared fuel cell can effectively avoid the collapse of the catalyst layer structure caused by carrier corrosion.
[0089] Example 2
[0090] A method for preparing a high entropy alloy aerogel for a fuel cell comprises the following steps:
[0091] S01. In an inert gas atmosphere, add a metal salt solution to a stabilizer and stir evenly to obtain a metal precursor mixed solution; the molar ratio of the metal salt to the stabilizer in the metal salt solution is 1:3;
[0092] S02, adding a reducing agent (excessive amount) to the metal precursor mixed solution of step S01, stirring and reacting at 60° C. for 2 h, and then aging for 24 h to obtain a metal nanoparticle sol;
[0093] S03, washing and drying the metal nanoparticle sol in step S02 to obtain a high entropy alloy aerogel for a fuel cell.
[0094] In step S01,
[0095] The inert gas is nitrogen.
[0096] The concentration of the metal salt solution is 2 mmol / L.
[0097] The metal salt solution includes five metal salts, and the molar ratio of metal ions in the five metal salts is 1:1:1:1:1.
[0098] The metal salt solution is a mixture of a platinum salt solution, a palladium salt solution, a gold salt solution, a nickel salt solution and a cobalt salt solution.
[0099] The salt solution of platinum is H2PtCl6·6H2O. The salt solution of palladium is H2PdCl4. The salt solution of gold is HAuCl4·3H2O. The salt solution of nickel is NiCl2. The salt solution of cobalt is CoCl2.
[0100] The stabilizer is citric acid.
[0101] The stirring time is 30min.
[0102] In step S02,
[0103] The reducing agent is NaHB4.
[0104] In step S03,
[0105] The washing is performed with water; the number of washing times is 6 times.
[0106] The drying is carried out by supercritical CO2 drying; the drying temperature is 35°C, the drying pressure is 7.5MPa, and the drying time is 3h.
[0107] The prepared high entropy alloy aerogel (Pt-Pd-Au-Ni-Co) for fuel cells has a particle size of 10nm to 50nm and a density of 0.13g / cm 3 , specific surface area 66.3m2 / g, half-wave potential 0.87V, mass specific activity up to 0.30A / cm 2 @0.9V Pt / g , the oxygen reduction electron transfer number is 3.80, and the half-wave potential drops by 5mV after 10,000 cycles of 1V to 1.5V.
[0108] The fuel cell prepared in this embodiment is prepared by replacing the catalyst layer with high entropy alloy aerogel and arranging it on both sides of the proton exchange membrane, and the other structural components of the fuel cell are conventional components and arranged in a conventional manner. The prepared fuel cell can effectively avoid the collapse of the catalyst layer structure caused by carrier corrosion.
[0109] Example 3
[0110] A method for preparing a high entropy alloy aerogel for a fuel cell comprises the following steps:
[0111] S01. In an inert gas atmosphere, add a metal salt solution to a stabilizer and stir evenly to obtain a metal precursor mixed solution; the molar ratio of the metal salt to the stabilizer in the metal salt solution is 1:3;
[0112] S02, adding a reducing agent (excessive amount) to the metal precursor mixed solution of step S01, stirring and reacting at 60° C. for 2 h, and then aging for 24 h to obtain a metal nanoparticle sol;
[0113] S03, washing and drying the metal nanoparticle sol in step S02 to obtain a high entropy alloy aerogel for a fuel cell.
[0114] In step S01,
[0115] The inert gas is nitrogen.
[0116] The concentration of the metal salt solution is 2 mmol / L.
[0117] The metal salt solution includes five metal salts, and the molar ratio of metal ions in the five metal salts is 1:1:1:1:1.
[0118] The metal salt solution is a mixture of a platinum salt solution, a palladium salt solution, a gold salt solution, a copper salt solution and a cobalt salt solution.
[0119] The salt solution of platinum is H2PtCl6·6H2O. The salt solution of palladium is H2PdCl4. The salt solution of gold is HAuCl4·3H2O. The salt solution of copper is CuCl2. The salt solution of cobalt is CoCl2.
[0120] The stabilizer is citric acid.
[0121] The stirring time is 30min.
[0122] In step S02,
[0123] The reducing agent is NaHB4.
[0124] In step S03,
[0125] The washing is performed with water; the number of washing times is 6 times.
[0126] The drying is carried out by supercritical CO2 drying; the drying temperature is 35°C, the drying pressure is 7.5MPa, and the drying time is 3h.
[0127] The prepared high entropy alloy aerogel (Pt-Pd-Au-Cu-Co) for fuel cells has a particle size of 10nm to 50nm and a density of 0.14g / cm 3 , specific surface area 68.5m 2 / g, half-wave potential 0.86V, mass specific activity up to 0.29A / cm 2 @0.9V Pt / g The oxygen reduction electron transfer number is 3.79, and the half-wave potential drops by 4mV after 10,000 cycles of 1V to 1.5V.
[0128] Comparative Example 1
[0129] A method for preparing an alloy aerogel comprises the following steps:
[0130] S01. In an inert gas atmosphere, the salt solutions of platinum, palladium and gold are stirred evenly to obtain a metal precursor mixed solution; S02. A reducing agent (excessive amount) is added to the metal precursor mixed solution of step S01, and the mixture is stirred at 60° C. for 1 hour, and then aged for 24 hours to obtain a metal nanoparticle sol;
[0131] S03, washing and drying the metal nanoparticle sol in step S02 to obtain an alloy aerogel.
[0132] In step S01,
[0133] The inert gas is nitrogen.
[0134] The concentration of the metal salt solution is 5 mmol / L.
[0135] The metal salt solution includes three metal salts, and the molar ratio of metal ions in the three metal salts is 1:1:1.
[0136] The metal salt solution is a mixture of a platinum salt solution, a palladium salt solution and a gold salt solution.
[0137] The salt solution of platinum is H2PtCl6·6H2O. The salt solution of palladium is H2PdCl4. The salt solution of gold is HAuCl4·3H2O.
[0138] The stirring time is 30min.
[0139] In step S02,
[0140] The reducing agent is ascorbic acid.
[0141] In step S03,
[0142] The washing is performed with water; the number of washing times is 6 times.
[0143] The drying is carried out by supercritical CO2 drying; the drying temperature is 35°C, the drying pressure is 7.5MPa, and the drying time is 3h.
[0144] The prepared fuel cell alloy aerogel (Pt-Pd-Au) has a particle size of 20nm to 60nm and a density of 0.15g / cm 3 , specific surface area 58.3m 2 / g, half-wave potential 0.83V, mass specific activity up to 0.28A / cm 2 @0.9V Pt / g The oxygen reduction electron transfer number is 3.76, and the half-wave potential drops by 6mV after 10,000 cycles of 1V to 1.5V.
[0145] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a high entropy alloy aerogel for a fuel cell, characterized in that: The steps include: S01. In an inert gas atmosphere, add a metal salt solution to a stabilizer, stir evenly, and obtain a metal precursor mixed solution; the molar ratio of the metal salt in the metal salt solution to the stabilizer is 1:(3-5); S02, adding a reducing agent to the metal precursor mixed solution of step S01, stirring and reacting at 50° C. to 80° C. for 1 h to 6 h, and then aging for 12 h to 24 h to obtain a metal nanoparticle sol; S03, washing and drying the metal nanoparticle sol in step S02 to obtain a high entropy alloy aerogel for a fuel cell; In step S01, the concentration of the metal salt solution is 1 mmol / L to 5 mmol / L; The metal salt solution is a mixture of at least five of a platinum salt solution, a palladium salt solution, a gold salt solution, a nickel salt solution, a copper salt solution and a cobalt salt solution, and the molar proportion of the metal ions in the five mixtures is 15% to 25% based on the sum of the molar numbers of the five mixtures as 100%; In step S01, the stabilizer is one of citric acid, sodium citrate, polyvinyl pyrrolidone and cyclohexane or a mixture of at least two thereof; In step S02, the reducing agent is one or a mixture of at least two of NaHB4, ascorbic acid and sodium hypophosphite.
2. The method for preparing a high entropy alloy aerogel for a fuel cell according to claim 1, characterized in that: The platinum salt solution is one or a mixed solution of at least two of H2PtCl6·6H2O, Na2PtCl6 and K2PtCl6; The palladium salt solution is one of H2PdCl4, Na2PdCl4 and K2PdCl4 or a mixture of at least two thereof; The gold salt solution is one of HAuCl4·3H2O, NaAuCl4 and KAuCl4 or a mixture of at least two thereof; The nickel salt solution is one or a mixture of two of Ni(NO3)2 and NiCl2; The copper salt solution is one or a mixture of two of Cu(NO3)2 and CuCl2; The cobalt salt solution is one or a mixture of two of Co(NO3)2 and CoCl2.
3. The method for preparing a high entropy alloy aerogel for a fuel cell according to claim 1, characterized in that: In step S01, the stirring time is 30 min to 60 min.
4. A high entropy alloy aerogel for a fuel cell, characterized in that: The method is prepared according to any one of claims 1 to 3.
5. A fuel cell, characterized in that: The fuel cell comprises a proton exchange membrane, and the high entropy alloy aerogel for a fuel cell according to claim 4 is arranged on a side of the proton exchange membrane.