A kind of frost-resistant concrete and production method thereof

By using penetrants and reinforcing agents in recycled aggregate concrete to fill gaps and enhance the surface structure, combined with air-entraining agents and butadiene-styrene copolymer emulsions, the problem of frost resistance of recycled aggregate concrete in freeze-thaw environments in cold areas is solved. It solves the problem of poor thawing cycle performance and significantly improves its freeze-thaw and crack resistance.

CN116177937BActive Publication Date: 2024-10-01JINAN SHENGHUA CONCRETE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310149571.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-10-01
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

Recycled aggregate concrete has poor resistance to freeze-thaw cycles in cold zone freeze-thaw environments and is prone to cracking, mainly due to moisture storage problems caused by its high water absorption rate and defects of multiple pores and cracks.

Method used

Adopt an enhanced recycled aggregate formula, including recycled aggregate, penetrant and reinforcing agent. The penetrant fills the gaps and the reinforcing agent enhances the surface and gap structure, reduces water absorption and improves strength. It combines air-entraining agent and butadiene-styrene. The copolymer emulsion regulates air bubbles and improves freeze-thaw cycle resistance.

Benefits of technology

It effectively reduces the water absorption rate of recycled aggregates, enhances its bonding strength with other raw materials, improves the freeze-thaw cycle resistance and crack resistance of concrete, and at the same time enhances the frost resistance by introducing air bubbles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004090281410000061
    Figure BDA0004090281410000061
  • Figure BDA0004090281410000071
    Figure BDA0004090281410000071
Patent Text Reader

Abstract

The present application relates to the field of building materials, and specifically discloses an antifreeze concrete and a production method thereof. The antifreeze concrete is composed of the following raw materials in parts by weight: 600-720 parts of reinforced recycled aggregate, 400-480 parts of natural stone, 600-800 parts of natural sand, 250-300 parts of cement, 50-100 parts of fly ash, 50-100 parts of mineral powder, 150-200 parts of water, and 3-5 parts of air entraining agent. The reinforced recycled aggregate includes recycled aggregate, penetrant and reinforcing agent, and the weight ratio of the recycled aggregate, penetrant and reinforcing agent is 20-40:2-4:1-2. The antifreeze concrete of the present application can be used for construction in cold areas, and has the advantage of strong antifreeze-thaw cycle ability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of building materials, and more specifically, to a frost-resistant concrete and a production method thereof. Background Art

[0002] Frost-resistant concrete is a type of concrete that has the durability to resist freeze-thaw cycles for a long time. By using frost-resistant concrete, the structural design can meet the specified frost resistance level.

[0003] If recycled aggregate concrete is used in construction, the recycled aggregate will absorb a large amount of water during the mixing process because of its high porosity and cracks.

[0004] For cold regions, when recycled concrete is used to cast buildings, the moisture stored in the recycled aggregate causes the concrete building to have poor resistance to freeze-thaw cycles, which can easily cause the concrete building to crack in a freeze-thaw environment. Summary of the invention

[0005] In order to improve the performance of recycled aggregate concrete in resisting freeze-thaw cycles, the present application provides a frost-resistant concrete and a production method thereof.

[0006] In a first aspect, the present application provides a frost-resistant concrete, which adopts the following technical solution:

[0007] A frost-resistant concrete is composed of the following raw materials in parts by weight: 600-720 parts of reinforced recycled aggregate, 400-480 parts of natural stone, 600-800 parts of natural sand, 250-300 parts of cement, 50-100 parts of fly ash, 50-100 parts of mineral powder, 150-200 parts of water, and 3-5 parts of air entraining agent. The reinforced recycled aggregate comprises recycled aggregate, a penetrant and a reinforcing agent, and the weight ratio of the recycled aggregate, the penetrant and the reinforcing agent is 20-40:2-4:1-2.

[0008] By adopting the above technical scheme, the penetrant is first used to penetrate the recycled aggregate, thereby filling the pores and gaps inside the recycled aggregate, effectively reducing the water absorption rate of the recycled aggregate, and the reinforcing agent is used to strengthen the recycled aggregate, which is mainly reflected in the filling support of the cracks and the reinforcement of the outer surface of the recycled aggregate, thereby effectively reducing the water entering the interior of the recycled aggregate and improving the strength of the recycled aggregate, making the recycled aggregate not easy to break during the freeze-thaw cycle process, and effectively improving the freeze-thaw cycle resistance of the concrete.

[0009] Preferably, the penetrant comprises water-absorbing resin powder, nano whiskers and lithium silicate solution, and the weight ratio of the water-absorbing resin powder, nano whiskers and lithium silicate solution is 3-5:1:16-34.

[0010] By adopting the above technical scheme, water-absorbent resin powder and nano whiskers are filled into the gap, and then the lithium silicate solution is used to penetrate it. The water-absorbent resin absorbs water to support the gap, while the nano whiskers enter the deep part of the gap with the lithium silicate solution to fill the deep part of the gap. After the lithium silicate is cured, the water-absorbent resin that absorbs water plays a role similar to a positioning pile in the gap, thereby improving the stability of the lithium silicate solidified material in the gap.

[0011] Preferably, the reinforcing agent comprises aramid fiber, aqueous polyurethane emulsion and rubber powder, and the weight ratio of the aramid fiber, aqueous polyurethane emulsion and rubber powder is 3 to 7:6 to 12:1.

[0012] By adopting the above technical scheme, aramid fibers are bonded to the surface of recycled aggregates through water-based polyurethane emulsion, one end of some aramid fibers is inserted into the gaps to combine with the lithium silicate solid. Rubber powder further fills the gaps and further fixes the aramid fibers inserted into the gaps. The rubber powder and aramid fibers mainly serve to increase the roughness of the surface of recycled aggregates, thereby enhancing the bonding strength between recycled aggregates and other raw materials and improving the crack resistance of concrete.

[0013] Preferably, the reinforced recycled aggregate is prepared by the following steps: the recycled aggregate is first stirred and mixed with water-absorbing resin powder and nano whiskers, then a lithium silicate solution is added and stirred, the mixture is allowed to stand in an environment of 60° C. for 2 hours, aramid fiber, rubber powder and aqueous polyurethane emulsion are added and mixed, and the mixture is cured at 60° C. for 24 hours to obtain the reinforced recycled aggregate.

[0014] By adopting the above technical scheme, the gaps in the recycled aggregate are first filled to reduce the water absorption rate of the recycled aggregate, and then the surface of the recycled aggregate is enhanced, wherein the aramid fiber and rubber powder are fixed by the water-based polyurethane emulsion, thereby improving the roughness of the enhanced recycled aggregate. The water-based polyurethane emulsion forms an external film to improve the freeze-thaw cycle resistance of the recycled aggregate, which is beneficial to improving the crack resistance of the recycled concrete.

[0015] Preferably, the recycled aggregate is first cleaned, and the specific steps are: immersing the recycled aggregate in a 2% by mass dilute hydrochloric acid solution, soaking for 12 hours, taking it out and treating it with clean water, repeating the operation 3 to 5 times, and finally taking it out and air-drying it for use.

[0016] By adopting the above technical solution, the original aged mortar on the surface of the recycled aggregate is cleaned with a dilute hydrochloric acid solution, thereby improving the physical properties of the recycled aggregate and cleaning the gaps at the same time, which is more conducive to the penetration and filling of the penetrant.

[0017] Preferably, the particle size grading of the reinforced recycled aggregate includes 15-20 mm and 9.5-15 mm, and the weight ratio between the two is 1:2; the particle size grading of the natural stone includes 9.5-15 mm and 4.75-9.5 mm, and the weight ratio between the two is 1:1.

[0018] By adopting the above technical solution, the gradation of the reinforced recycled aggregate and the natural stone is adjusted, and the natural stone replaces part of the reinforced recycled aggregate, so that the strength of the reinforced recycled aggregate concrete is improved.

[0019] Preferably, the invention further comprises 3 to 5 parts of a foam leveler and 12 to 36 parts of a butadiene-styrene copolymer emulsion.

[0020] By adopting the above technical solution, when the air entraining agent generates bubbles in the concrete, the foam leveling agent can adjust the pores, and at the same time the butadiene-styrene copolymer emulsion strengthens the bubbles and improves the stability of the bubbles.

[0021] In a second aspect, the present application provides a method for producing frost-resistant concrete, which adopts the following technical solution:

[0022] A method for producing frost-resistant concrete comprises the following steps: mixing reinforced recycled aggregate, natural stone, natural sand, cement, fly ash, mineral powder and water evenly, adding air entraining agent for foaming and pouring.

[0023] By adopting the above technical solution, the raw materials except the air entraining agent are first mixed, and then the air entraining agent is added for foaming to introduce bubbles into the concrete, thereby effectively improving the concrete's ability to resist freeze-thaw cycles.

[0024] In summary, this application has the following beneficial effects:

[0025] 1. Since the present invention first fills the internal gaps of the recycled aggregate and then seals the gaps from the outside, the water absorption rate of the recycled aggregate is effectively reduced, and by strengthening the surface of the recycled aggregate, the bonding strength between the recycled aggregate and other raw materials is increased, thereby improving the freeze-thaw cycle resistance of the concrete.

[0026] 2. In this application, the recycled aggregate is first cleaned with a dilute hydrochloric acid solution, which effectively reduces the impact of the original aging mortar on the performance of the recycled aggregate and reduces the water absorption rate of the recycled aggregate.

[0027] 3. In this application, the air entraining agent increases the air volume in the concrete, and the air bubbles can improve the frost resistance of the concrete, while the foam leveling agent and butadiene-styrene copolymer emulsion adjust the pore size, enhance the air bubble strength, and effectively improve the freeze-thaw resistance of the concrete. DETAILED DESCRIPTION

[0028] The bulk density of recycled aggregate in this application is 1284kg / m 3, water absorption rate is 8%, crushing index is 16.3%, particle size is 8-20mm; natural stone is purchased from the market, natural sand particle size is 0.075-4.75mm, purchased from the market. Cement is P.Ⅱ42.5 silicate cement, purchased from the market; fly ash is grade Ⅱ fly ash, purchased from the market; mineral powder is grade S95, purchased from the market; air entraining agent is sodium dodecyl sulfate, purchased from the market; water-absorbing resin powder fineness is 800 mesh, purchased from the market; nano whiskers are silicon carbide whiskers with a fineness of 200nm, purchased from the market; lithium silicate solution is a lithium silicate aqueous solution with a mass fraction of 20%, purchased from the market; aramid fiber length is 2-4cm, purchased from the market; water-based polyurethane emulsion is purchased from the market; rubber powder fineness is 200 mesh, purchased from the market; foam leveling agent is purchased from the market; butadiene-styrene copolymer emulsion is purchased from the market.

[0029] The present application is further described in detail below with reference to the embodiments.

[0030] Preparation Example

[0031] Preparation Example 1

[0032] This preparation example discloses a reinforced recycled aggregate, which is prepared by the following steps:

[0033] 200 kg of recycled aggregate was first mixed with 3 kg of absorbent resin powder and 1 kg of silicon carbide whisker, and then 16 kg of lithium silicate solution was added and stirred, and the mixture was allowed to stand at 60°C for 2 hours. Then 7 kg of aramid fiber, 1 kg of rubber powder and 12 kg of aqueous polyurethane emulsion were added and mixed, and the mixture was cured at 60°C for 24 hours to obtain reinforced recycled aggregate.

[0034] Preparation Example 2

[0035] This preparation example discloses a reinforced recycled aggregate, which is prepared by the following steps:

[0036] 300 kg of recycled aggregate was first mixed with 4 kg of absorbent resin powder and 1 kg of silicon carbide whisker, and then 25 kg of lithium silicate solution was added and stirred, and the mixture was allowed to stand at 60°C for 2 hours. Then 5 kg of aramid fiber, 1 kg of rubber powder and 9 kg of aqueous polyurethane emulsion were added and mixed, and the mixture was cured at 60°C for 24 hours to obtain reinforced recycled aggregate.

[0037] Preparation Example 3

[0038] This preparation example discloses a reinforced recycled aggregate, which is prepared by the following steps:

[0039] 400 kg of recycled aggregate was first stirred and mixed with kg of absorbent resin powder and kg of silicon carbide whisker, and then kg of lithium silicate solution was added and stirred and mixed, and allowed to stand at 60°C for 2 hours. Then 7 kg of aramid fiber, 1 kg of rubber powder and 12 kg of aqueous polyurethane emulsion were added and mixed, and cured at 60°C for 24 hours to obtain reinforced recycled aggregate.

[0040] Preparation Example 4

[0041] This preparation example discloses a reinforced recycled aggregate, which differs from preparation example 2 in that:

[0042] First, immerse the recycled aggregate in a 2% mass fraction dilute hydrochloric acid solution, take it out after soaking for 12 hours, treat it with clean water, repeat the operation 3 times, finally take it out and air-dry it for use, and then mix it with other raw materials to make reinforced recycled aggregate.

[0043] Preparation Example 5

[0044] This preparation example discloses a reinforced recycled aggregate, which differs from preparation example 2 in that:

[0045] First, immerse the recycled aggregate in a 2% mass fraction dilute hydrochloric acid solution, take it out after soaking for 12 hours, treat it with clean water, repeat the operation 5 times, finally take it out and air-dry it for use, and then mix it with other raw materials to make reinforced recycled aggregate.

[0046] Preparation Example 6

[0047] This preparation example discloses a reinforced recycled aggregate, which differs from preparation example 2 in that:

[0048] Aramid fiber, rubber powder and water-based polyurethane emulsion were not used to reinforce the filled recycled aggregate.

[0049] Preparation Example 7

[0050] This preparation example discloses a reinforced recycled aggregate, which differs from preparation example 2 in that:

[0051] The recycled aggregate was not filled with water-absorbent resin powder, nano whiskers and lithium silicate solution.

[0052] Example

[0053] Example 1

[0054] This embodiment discloses a frost-resistant concrete, which is prepared by the following steps:

[0055] Take 600kg of the reinforced recycled aggregate prepared in Preparation Example 1, 400kg of natural stone, 600kg of natural sand, 250kg of cement, 50kg of fly ash, 50kg of mineral powder and 150kg of water and stir and mix them evenly. The reinforced recycled aggregate includes two particle sizes of 15-20mm and 9.5-15mm, and the weight ratio of the two particle sizes is 1:2. The natural stone includes two particle sizes of 9.5-15mm and 4.75-9.5mm, and the weight ratio of the two particle sizes is 1:1. Then add 3kg of air entraining agent for foaming and pouring.

[0056] Example 2

[0057] This embodiment discloses a frost-resistant concrete, which is prepared by the following steps:

[0058] Take 660kg of the reinforced recycled aggregate prepared in Preparation Example 2, 440kg of natural stone, 700kg of natural sand, 275kg of cement, 75kg of fly ash, 75kg of mineral powder and 175kg of water and stir and mix them evenly. The reinforced recycled aggregate includes two particle sizes of 15-20mm and 9.5-15mm, and the weight ratio of the two particle sizes is 1:2. The natural stone includes two particle sizes of 9.5-15mm and 4.75-9.5mm, and the weight ratio of the two particle sizes is 1:1. Then add 4kg of air entraining agent for foaming and pouring.

[0059] Example 3

[0060] This embodiment discloses a frost-resistant concrete, which is prepared by the following steps:

[0061] Take 720kg of the reinforced recycled aggregate prepared in Preparation Example 3, 480kg of natural stone, 800kg of natural sand, 300kg of cement, 100kg of fly ash, 100kg of mineral powder and 200kg of water and stir and mix them evenly. The reinforced recycled aggregate includes two particle sizes of 15-20mm and 9.5-15mm, and the weight ratio of the two particle sizes is 1:2. The natural stone includes two particle sizes of 9.5-15mm and 4.75-9.5mm, and the weight ratio of the two particle sizes is 1:1. Then add 5kg of air entraining agent for foaming and pouring.

[0062] Example 4

[0063] This embodiment discloses a frost-resistant concrete, which is different from the embodiment 2 in that:

[0064] The reinforced recycled aggregate was prepared in Preparation Example 4.

[0065] Example 5

[0066] This embodiment discloses a frost-resistant concrete, which is different from the embodiment 2 in that:

[0067] The reinforced recycled aggregate was prepared in Preparation Example 5.

[0068] Example 6

[0069] This embodiment discloses a frost-resistant concrete, which is different from the embodiment 2 in that:

[0070] 3 kg of foam stabilizer and 12 kg of butadiene-styrene copolymer emulsion were also added.

[0071] Example 7

[0072] This embodiment discloses a frost-resistant concrete, which is different from the embodiment 2 in that:

[0073] 4 kg of foam stabilizer and 24 kg of butadiene-styrene copolymer emulsion were also added.

[0074] Example 8

[0075] This embodiment discloses a frost-resistant concrete, which is different from the embodiment 2 in that:

[0076] 5 kg of foam stabilizer and 36 kg of butadiene-styrene copolymer emulsion were also added.

[0077] Example 9

[0078] This embodiment discloses a frost-resistant concrete, which is different from Embodiment 2 in that no water-absorbing resin powder is added.

[0079] Example 10

[0080] This embodiment discloses a frost-resistant concrete, which is different from Embodiment 2 in that silicon carbide whiskers are not added.

[0081] Embodiment 11

[0082] This embodiment discloses a frost-resistant concrete, which is different from the embodiment 2 in that:

[0083] No water-absorbing resin powder and silicon carbide whiskers are added.

[0084] Comparative Example

[0085] Comparative Example 1

[0086] This comparative example discloses a frost-resistant concrete, which is different from Example 2 in that:

[0087] The reinforced recycled aggregate was prepared in Preparation Example 6.

[0088] Comparative Example 2

[0089] The reinforced recycled aggregate was prepared in Preparation Example 7.

[0090] Comparative Example 3

[0091] The reinforced recycled aggregate prepared in Preparation Example 2 was replaced by recycled aggregate.

[0092] Performance testing

[0093] According to GB / T 50081-2002 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete", the performance test is carried out. The specific test items are as follows:

[0094] 6. Compressive strength test.

[0095] According to GB / T 50082-2009 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete", the performance test is carried out. The specific test items are as follows:

[0096] 4 Antifreeze test 4.2 Rapid freezing method is used to detect the number of rapid freezing and thawing cycles of concrete.

[0097] Table 1 Performance test data table

[0098]

[0099]

[0100] It can be seen from Example 2 and Comparative Examples 1 to 3 and Table 1 that the internal gaps of the recycled aggregate are first filled and then sealed from the outside, which effectively reduces the water absorption rate of the recycled aggregate, and by strengthening the surface of the recycled aggregate, the bonding strength between the recycled aggregate and other raw materials is increased, thereby improving the compressive strength of the concrete and the freeze-thaw cycle resistance of the concrete.

[0101] It can be seen from Example 2, Example 4 and Example 5 and Table 1 that the recycled aggregate is first cleaned with a dilute hydrochloric acid solution, which effectively reduces the influence of the original aging mortar on the performance of the recycled aggregate and reduces the water absorption rate of the recycled aggregate, thereby improving the freeze-thaw cycle resistance of the concrete.

[0102] It can be seen from Example 2, Examples 6 to 8 and Table 1 that the air entraining agent increases the air volume in the concrete, and the bubbles can improve the frost resistance of the concrete, while the foam leveling agent and butadiene-styrene copolymer emulsion adjust the pore size, enhance the bubble strength, and effectively improve the freeze-thaw resistance of the concrete.

[0103] It can be seen from Example 2, Examples 9 to 11 and Table 1 that the water-absorbent resin powder and the nano whiskers are filled into the gap, and then the lithium silicate solution is used to penetrate it. The water-absorbent resin absorbs water to support the gap, and the nano whiskers enter the deep part of the gap with the lithium silicate solution to fill the deep part of the gap. After the lithium silicate is cured, the water-absorbent resin after absorbing water plays a role similar to that of a positioning pile in the gap, thereby improving the stability of the lithium silicate cured product in the gap, effectively reducing the water absorption rate of the reinforced recycled aggregate, and improving the freeze-thaw resistance of the concrete.

[0104] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A frost-resistant concrete, It is characterized in that The invention is composed of the following raw materials in parts by weight: 600-720 parts of reinforced recycled aggregate, 400-480 parts of natural stone, 600-800 parts of natural sand, 250-300 parts of cement, 50-100 parts of fly ash, 50-100 parts of mineral powder, 150-200 parts of water, and 3-5 parts of air entraining agent. The reinforced recycled aggregate includes recycled aggregate, penetrant and reinforcing agent, and the weight ratio of the recycled aggregate, penetrant and reinforcing agent is 20-40:2-4:1-2. The penetrant comprises water-absorbing resin powder, nano whiskers and lithium silicate solution, wherein the weight ratio of the water-absorbing resin powder, nano whiskers and lithium silicate solution is 3-5:1:16-34; The reinforcing agent comprises aramid fiber, water-based polyurethane emulsion and rubber powder, wherein the weight ratio of the aramid fiber, water-based polyurethane emulsion and rubber powder is 3-7:6-12:1; The invention also comprises 3 to 5 parts of a foam leveler and 12 to 36 parts of a butadiene-styrene copolymer emulsion.

2. The frost-resistant concrete according to claim 1, It is characterized in that The reinforced recycled aggregate is prepared by the following steps: the recycled aggregate is first stirred and mixed with water-absorbing resin powder and nano whiskers, then a lithium silicate solution is added and stirred, the mixture is allowed to stand in an environment of 60° C. for 2 hours, aramid fiber, rubber powder and water-based polyurethane emulsion are added and mixed, and the mixture is cured at 60° C. for 24 hours to obtain the reinforced recycled aggregate.

3. The frost-resistant concrete according to claim 2, It is characterized in that The recycled aggregate is first cleaned, and the specific steps are: immersing the recycled aggregate in a 2% by mass dilute hydrochloric acid solution, soaking for 12 hours, taking it out and treating it with clean water, repeating the operation 3 to 5 times, and finally taking it out and air-drying it for use.

4. The frost-resistant concrete according to claim 1, It is characterized in that The reinforced recycled aggregate particle size grading includes 15-20 mm and 9.5-15 mm, and the weight ratio between the two is 1:

2. The natural stone grading particle size includes 9.5-15 mm and 4.75-9.5 mm, and the weight ratio between the two is 1:

1.

5. The method for producing frost-resistant concrete according to any one of claims 1 to 4, It is characterized in that The following steps are involved: The reinforced recycled aggregate, natural stone, natural sand, cement, fly ash, mineral powder and water are mixed evenly, and then air entraining agent is added for foaming and pouring.