A fullerene pyrrolidine derivative and its preparation method and application
By preparing fullerene pyrrolidine derivatives as catalyst supports and loading Cu nanoparticles, the problem of low catalytic activity of existing fullerene C60 derivative-supported copper catalysts in the oxidation of benzyl alcohol was solved, achieving high catalytic efficiency and good product selectivity.
Patent Information
- Application Number
- CN202310249781.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-03-15
AI Technical Summary
Existing copper catalysts supported on fullerene C60 derivatives exhibit low catalytic activity, low conversion rate, and poor product selectivity in the oxidation of benzyl alcohol, and the catalytic mechanism is not fully understood.
Fullerene pyrrolidine derivatives were prepared as catalyst supports by synthesizing N-methyl-2-[3',4'-bis(5”-bromopentoxyphenyl)phenyl]-3,4-fullerene pyrrolidine or N-methyl-2-[3'-hydroxy-4'-bromopentoxyphenyl]-3,4-fullerene pyrrolidine and loading Cu nanoparticles for catalytic oxidation of benzyl alcohol.
It improves catalytic efficiency and selectivity, and the yield can still be maintained above 93% after the catalyst is recycled 5 times, with stable catalytic activity.
Smart Images

Figure CN116178244B_ABST
Abstract
Description
Technical Field
[0001] The invention provides a fullerene derivative and a preparation method thereof, as well as application of the fullerene derivative as a catalyst carrier for catalyzing the oxidation of benzyl alcohol. Background Art
[0002] Fullerene is the third allotrope of carbon. Due to its special structure, it has shown a wide range of application prospects in chemistry, biology, materials science, medicine and other fields. The most representative one is C 60 It has unique biological activities in anti-HIV virus, inhibiting cancer cell proliferation, scavenging free radicals, antibacterial, anti-oxidant, causing DNA cleavage, and acting as a drug carrier. 60 The poor solubility in polar solvents and unsatisfactory targeting limit its application in the biomedical field. Therefore, it is necessary to prepare C with special optical and electrical properties, good solubility and targeting specificity. 60 Derivatives are of great significance for exploring their biological activities and expanding new fullerene-based materials in the future.
[0003] Michele Maggini first reported the use of sarcosine, formaldehyde and C 60 Reflux in toluene to obtain N-methylfullerene pyrrolidine derivatives. In organic catalytic hydrogenation reactions, hydrogenation catalysts with high catalytic activity are the key to the reaction. Currently, most commonly used oxidation catalysts in industry are heterogeneous catalysts, especially supported heterogeneous catalysts. For example, in the catalytic oxidation reaction of benzyl alcohol to benzaldehyde, a commonly used catalyst is a heterogeneous catalyst copper, such as reduced graphene oxide supported copper, cerium dioxide supported copper, metal organic framework material (MOF) supported copper, etc. These catalysts have good advantages in catalytic activity, reaction conversion rate and product selectivity. At the same time, the catalyst has the characteristics of simple preparation process, cheap and easy to obtain copper salt raw materials, and is the main direction of heterogeneous catalyst research at this stage.
[0004] For carrier-supported copper catalysts, activated carbon, carbon nanotubes, titanium dioxide, ferroferric oxide, zeolite imidazolate framework materials (ZIF), covalent organic framework materials (COF), artificial fiber carbon and other carrier materials are relatively common carriers. In the catalytic reaction, the copper on the surface is only the active center, and the carrier plays a great role, and the carbon carrier is crucial for promoting the contact between the reactants and the active centers. In addition, the dispersion and particle size of copper and the interaction between copper and the carrier are also important factors affecting the catalytic oxidation reaction. However, the existing carrier-supported nano-copper catalysts still have the disadvantages of low catalytic activity, low reaction conversion rate, and poor product selectivity. At the same time, the structure and catalytic mechanism of this type of catalyst have not been fully studied.
[0005] In recent years, carbon nanomaterials loaded with metal catalysts have attracted extensive attention. These carbon nanomaterials include fullerenes, carbon nanotubes and graphene. They have strong delocalized π electrons, significant conjugation effects, and good thermal conductivity, mechanical properties, gas adsorption and monitoring properties, etc., which can improve catalytic activity, reaction conversion rate and product selectivity in the catalytic process.
[0006] CN103396354A discloses a method for synthesizing a fullerene pyrrolidine derivative, which uses fullerene, organic halide and α-amino acid as raw materials, dimethyl sulfoxide as a catalyst, and reacts in an organic solvent to generate a fullerene pyrrolidine derivative. This method has cheap and readily available raw materials, high yield, simple operation, and is suitable for large-scale production of fullerene pyrrolidine derivatives. Its preparation method is different from that of the present invention, and it does not disclose whether the obtained fullerene pyrrolidine derivative can be used for carbon material-loaded metal nanocatalysts, and it does not disclose whether the above-mentioned fullerene pyrrolidine can be used for fullerene C 60 A method for preparing N-methyl-2-(3-methoxy-4-hydroxyphenyl)-3,4-fullerene pyrrolidine comprises the following steps: (1) 60 The powder is dissolved in a non-polar solvent to obtain a solution; (2) sarcosine and vanillin are added to the solution obtained in step (1), and then heated and refluxed; (3) after the reflux, the mixed solution is cooled, and toluene is removed to obtain a solid product; (4) the solid product obtained in step (3) is eluted with a chromatography column; (5) the eluted product solution is free of solvent, washed, and dried to obtain the target product. The above patent discloses a method for preparing the fullerene pyrrolidine, and the main raw material used is C 60 The above patent does not disclose whether the obtained fullerene pyrrolidine can be used in the preparation of carbon material supported metal nanocatalysts and its specific preparation method, nor does it disclose whether the above fullerene pyrrolidine can be used in the preparation of fullerene C 60 In the derivative-loaded copper nanocatalyst, although it is also fullerene pyrrolidine, the properties and uses of different fullerene pyrrolidines are also very different.
[0007] Therefore, it is necessary to prepare a method that can be applied to fullerene C 60 The derivative-loaded copper nanocatalyst is used to catalyze the oxidation of benzyl alcohol to prepare benzaldehyde, and the catalytic oxidation of benzyl alcohol has a high yield, good selectivity and recycling performance. Summary of the invention
[0008] The invention relates to a method for preparing a fullerene pyrrolidine derivative. The method comprises the following steps: firstly, 3,4-di(5'-bromopentyloxy)benzaldehyde (A) or 3-hydroxy-4-bromopentyloxybenzaldehyde (B) is synthesized from dihydroxybenzaldehyde; then N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenyl pyrrolidine (C) is synthesized from 3,4-di(5'-bromopentyloxy)benzaldehyde (A), or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenyl pyrrolidine (D) is synthesized from 3-hydroxy-4-bromopentyloxybenzaldehyde (B).
[0009] The preparation method of the above-mentioned fullerene pyrrolidine derivative is as follows:
[0010] (a) Synthesis of 3,4-bis(5'-bromopentyloxy)benzaldehyde (A) or 3-hydroxy-4-bromopentyloxybenzaldehyde (B);
[0011] Specifically, under the protection of inert gas, dihydroxybenzaldehyde and Br(CH 2 ) 5 Br, K 2 CO 3 Dissolve, heat, stir and reflux; after cooling to room temperature, filter and concentrate the reaction solution; then separate the concentrated solution by column chromatography to obtain intermediate products 3,4-di(5'-bromopentyloxy)benzaldehyde (A) and 3-hydroxy-4-bromopentyloxybenzaldehyde (B).
[0012] The above intermediate products 3,4-di(5'-bromopentyloxy)benzaldehyde (A) and 3-hydroxy-4-bromopentyloxybenzaldehyde (B) can be obtained under different eluent conditions. For example, they can be:
[0013] When the eluent is V 乙酸乙酯 :V 石油醚 =1:5, 3,4-di(5'-bromopentyloxy)benzaldehyde (A) was separated; when the eluent was V 乙酸乙酯 :V 石油醚 =1:4, 3-hydroxy-4-bromopentyloxybenzaldehyde (B) was separated.
[0014] (b) Synthesis of N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (C):
[0015] Under inert gas protection, C 60After dissolving and stirring, 3,4-di(5'-bromopentyloxy)benzaldehyde (A) and sarcosine are added, and the temperature is raised to reflux and stirred evenly; after cooling to room temperature, the reaction solution is concentrated; and then the concentrated solution is separated by column chromatography. When the eluent is pure dichloromethane, N-methyl-2-[3',4'-di(5'-bromopentyloxy)phenyl]-3,4-fullerenepyrrolidine (C) is separated;
[0016] Further, it can be: under the protection of inert gas, 0.01-0.08 molC 60 Dissolve in 20-80 mL of freshly distilled toluene solution, stir for 0.5-3 h, add 0.1-0.5 mol of 3,4-di(5'-bromopentyloxy)benzaldehyde (A) and 0.1-0.3 mol of sarcosine, heat to 90-130°C and reflux with stirring for 1-3 h; after cooling to room temperature, concentrate the reaction solution; then separate the concentrated solution by column chromatography to separate N-methyl-2-[3',4'-di(5'-bromopentyloxy)phenyl]-3,4-fullerenepyrrolidine (C);
[0017] (b') Synthesis of N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine (D):
[0018] Under inert gas protection, C 60 After dissolving and stirring, 3-hydroxy-4-bromopentyloxybenzaldehyde (B) and sarcosine were added, and the temperature was raised to reflux and stirred evenly; after cooling to room temperature, the reaction solution was concentrated; and the concentrated solution was separated by column chromatography. When the eluent was V 石油醚 :V 乙酸乙酯 =4:1, N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine (D) was isolated.
[0019] Further, it can be: under the protection of inert gas, 0.05-0.25 molC 60 Dissolve in 50-100 mL of freshly distilled toluene solution, stir for 0.5-3 h, add 0.2-0.8 mol of 3-hydroxy-4-bromopentyloxybenzaldehyde (B) and 0.2-0.5 mol of sarcosine, heat to 90-130°C, reflux and stir for 1-3 h; after cooling to room temperature, concentrate the reaction solution; then separate the concentrate by column chromatography to separate N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine (D).
[0020] The present invention also relates to the use of the fullerene pyrrolidine derivative as a catalyst carrier; specifically, it can be the use of the fullerene pyrrolidine derivative as a catalyst carrier to catalyze the oxidation of benzyl alcohol.
[0021] As a catalyst carrier, for example, it can be N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine) supported Cu nanoparticle catalyst. The preparation method of the catalyst is:
[0022] (1) adding deionized water to N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine), and ultrasonically treating the mixture to uniformly disperse the mixture;
[0023] (2) dissolving cupric chloride in deionized water, adding the solution to the dispersion, and stirring to uniformly mix N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine) and cupric chloride;
[0024] (3) Ammonia borane (BH 3 ·NH 3 ) solution is slowly added to the above mixed solution for reduction, heated under stirring, so that the color of the mixed solution gradually changes from dark green to black, and then the solution is allowed to stand at room temperature;
[0025] (4) The mixed solution is centrifuged to remove the upper solution, and the lower precipitate after centrifugation is dried to obtain N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine)-loaded Cu nanoparticle catalyst.
[0026] Furthermore, the preparation method of the catalyst is:
[0027] (1) Add 80-120 mL of deionized water to 30-50 mg of N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine, and perform ultrasonic treatment at 30-70° C. for 1.5-3.5 h to uniformly disperse the mixture;
[0028] (2) In a 60-90°C oil bath, under magnetic stirring, add 10-30 mg of copper chloride (CuCl 2 ·2H 2O) is dissolved in 10-30 mL of deionized water, added to the above dispersion, and stirred to uniformly mix N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine and cupric chloride;
[0029] (3) Add 1-10 mL of 0.5-2.0 mmol / L ammonia borane (BH 3 ·NH 3 ) solution is slowly added to the above mixed solution for reduction, and heated in an oil bath at 60-90°C for 1-5h under vigorous magnetic stirring to gradually change the color of the mixed solution from dark green to black, and then the solution is allowed to stand at room temperature for 12-24h;
[0030] (4) The mixed solution is centrifuged to remove the upper solution, and the lower precipitate after centrifugation is dried to obtain N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenyl pyrrolidine or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenyl pyrrolidine-loaded Cu nanoparticle catalyst.
[0031] The catalyst can be stored in a desiccator for future use.
[0032] The Cu nanoparticle catalyst supported on N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine) obtained above is used to catalyze the oxidation of benzyl alcohol;
[0033] For example, the specific reaction steps can be as follows:
[0034] (1) Add benzyl alcohol, the above catalyst, and deionized water into a reaction flask, and continue to pass O 2 , placing the reaction bottle in an oil bath, raising the temperature (e.g., to 110° C.), allowing the reaction to fully proceed (e.g., 12 h), stopping the reaction, and characterizing and analyzing the product using a gas chromatography-mass spectrometer (GC-MS);
[0035] (2) The two catalysts were recycled for 5 times to investigate their recycling rates. The experiment showed that the N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine-loaded Cu nanoparticles and N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine-loaded Cu nanoparticles had high catalytic efficiency and good selectivity when catalyzing the oxidation of benzyl alcohol. Moreover, the yield of the catalyst could be maintained at a high ratio after multiple recycling, and the catalytic activity of the two catalysts was relatively stable.
[0036] Beneficial effects of the present invention:
[0037] 1. The fullerene pyrrolidine derivative prepared by the present invention has a simple preparation method; the prepared N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenyl pyrrolidine or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenyl pyrrolidine can be used as a metal nanoparticle catalyst carrier;
[0038] 2. When the fullerene pyrrolidine-loaded Cu nanoparticles prepared in the present invention catalyze the oxidation of benzyl alcohol, the catalytic efficiency is high and the selectivity is good. After the catalyst is recycled for 5 times, the yield can be maintained at more than 93%. The catalytic activity of the two catalysts is relatively stable. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0040] Figure 1 It is a synthetic route for fullerene pyrrolidine derivatives;
[0041] Figure 2 Transmission electron microscopy images of (a) N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine-loaded Cu nanoparticles and (b) N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine-loaded Cu nanoparticles;
[0042] Figure 3 The chemical equation for the catalytic oxidation of benzyl alcohol;
[0043] Figure 4 3,4-bis(5'-bromopentyloxy)benzaldehyde (A) 1 H-NMR spectrum;
[0044] Figure 5 is the infrared spectrum of 3,4-bis(5'-bromopentyloxy)benzaldehyde (A);
[0045] Figure 6 3-Hydroxy-4-bromopentyloxybenzaldehyde (B) 1 H-NMR spectrum;
[0046] Figure 7 is the infrared spectrum of 3-hydroxy-4-bromopentyloxybenzaldehyde (B);
[0047] Figure 8 N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (C) 1 H-NMR spectrum;
[0048] Fig. 9 is the infrared spectrum of N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (C);
[0049] Fig.10 N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine (D) 1 H-NMR spectrum;
[0050] Fig.11 This is the infrared spectrum of N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine (D). DETAILED DESCRIPTION
[0051] To facilitate understanding of the present invention, various exemplary embodiments of the present invention are now described in detail. This detailed description should not be regarded as a specific limitation of the present invention, but should be understood as a more detailed description of certain aspects, features and embodiments of the present invention.
[0052] Example 1
[0053] Raw materials: 3,4-dihydroxybenzaldehyde (AR from Shanghai Experimental Reagent Co., Ltd.); 1,5-dibromopentane (AR from Shanghai Experimental Reagent Co., Ltd.); potassium carbonate (AR from Shanghai Experimental Reagent Co., Ltd.); deuterated chloroform (AR from AlfaAesar); acetone (AR from Shanghai Experimental Reagent Co., Ltd.); petroleum ether (AR boiling range of 60-90℃ and 30-60℃ from Shanghai Experimental Reagent Co., Ltd. and Beijing Changhai Chemical Plant respectively); (n-Bu) 4 N + F - (ARAlfa Aesar); Toluene (AR Shanghai Testing Reagent Co., Ltd.); C 60 (99%); sarcosine (98% provided by Alfa Aesar).
[0054] A method for preparing a fullerene pyrrolidine derivative, such as Figure 1 As shown, the reaction process includes the following steps:
[0055] (a) Synthesis of 3,4-di(5'-bromopentyloxy)benzaldehyde (A) and 3-hydroxy-4-bromopentyloxybenzaldehyde (B):
[0056] Under argon (Ar) protection, 3,4-dihydroxybenzaldehyde 2.7979 g (20.3 mmol), Br (CH 2 ) 5 Br13mL (96.0mmol), K 2 CO 3 2.79 g (20 mmol) was dissolved in 30 mL acetone (freshly distilled) and stirred at 56 °C for 12 h. After cooling to room temperature, the reaction solution was filtered and concentrated. The concentrate was then separated by column chromatography. When the eluent was V 乙酸乙酯 :V 石油醚 =1:5, 3.24gA was separated, with a yield of about 34%; Figure 4 As shown, 1 H-NMR (CDCl 3 ),δ:1.7–2.02 (12H, multiplet) corresponds to the aliphatic hydrogen in the compound, 3.40–3.45 (4H, triplet) corresponds to –CH 2 Hydrogen in Br, 4.01–4.05 (4H, triplet) corresponds to –OCH 2 The hydrogens of 6.96–7.64 (3H, multiple peaks) correspond to the hydrogens on the benzene ring, and 9.85 (1H, single peak) corresponds to the hydrogens in –CHO. Figure 5 As shown, IR (KBr): 3449cm -1 and 3333cm -1 is the absorption peak of water; 3078cm -1 The stretching vibration of C–H on the benzene ring; 2862 cm -1 and 2762cm -1 1678cm is the stretching vibration of C–H in the aldehyde group; and 1840 is the stretching vibration of C=O in the aldehyde group. -1 、1581cm -1 、1512cm -1 and 1435cm -1 It is the stretching vibration of C=C on the benzene ring. 864cm -1 、806cm -1 、752cm -1 It is the bending vibration of C–H on the benzene ring. -1There are more peaks in the range of 2 –C–H bending vibration and –O–CH 2 - and –CH 2 Vibration of C–H in –Br.
[0057] When the eluent is V 乙酸乙酯 :V 石油醚 =1:4, 1.8551 g of by-product B was separated, with a yield of about 29.8%. Figure 6 As shown, 1 H-NMR (CDCl 3 ),δ:1.7–2.02 (6H, multiplet) corresponds to the aliphatic hydrogen in the compound, 3.40–3.45 (2H, triplet) corresponds to –CH 2 Hydrogen in Br, 4.01–4.05 (2H, triplet) corresponds to –OCH 2 The peaks at 6.96–7.64 (3H, multiple peaks) correspond to the hydrogen on the benzene ring, and 9.85 (1H, single peak) correspond to the hydrogen in –CHO. There is a stronger peak at 5.78, which corresponds to the hydrogen of the hydroxyl group attached to the benzene ring. Figure 7 As shown, IR (KBr) 3340cm -1 、3078cm -1 、2862cm -1 、2762cm -1 、1840cm -1 、1678cm -1 、1581cm -1 、1512cm -1 、1435cm -1 、864cm -1 、806cm -1 、752cm -1 .
[0058] Its peak shape is basically similar to the infrared spectrum of A. The difference is that B has a peak at 3340cm -1 There is an absorption peak at , which is the stretching vibration of O–H on the benzene ring.
[0059] (b) Synthesis of N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (C):
[0060] Under Ar protection, 36.3 mg C 60(0.05mmol) was dissolved in 40mL of freshly distilled toluene, stirred for 1h, and then 124.5mg (0.34mmol) of compound A and 14.1mg (0.16mmol) of sarcosine were added, and refluxed and stirred at 114°C for 2.5h. After cooling to room temperature, the reaction solution was concentrated. The concentrate was then separated by column chromatography. When the eluent was pure dichloromethane, about 15.3mg of N-methyl-2-[3',4'-di(5'-bromopentyloxy)phenyl]-3,4-fullerenepyrrolidine (C) was separated, with a yield of about 25.6%. Figure 8 As shown, 1 H-NMR (CDCl 3 ),δ:1.29–1.80 (12H, multiple peaks) corresponding to aliphatic hydrogen in the compound, 3.40–3.45 (4H, triplet) corresponding to –CH 2 Br hydrogen, 4.01–4.05 (4H, triplet) corresponds to –OCH 2 4.23–4.26 (1H, doublet) correspond to the hydrogen at the 2-position of pyrrolidine, 4.86–5.00 (2H, triplet) correspond to the hydrogen at the 5-position of pyrrolidine, and 2.38 (3H, singlet) corresponds to –CH 3 Hydrogen on the benzene ring (due to C 60 The dispersed conjugation effect causes the two hydrogen atoms to shift to above 7.0, which is exactly the same as CDCl 3 The solvent peaks of Fig. 9 As shown, IR (KBr) 525cm -1 、1427cm -1 、3078cm -1 、2862cm -1 、2762cm -1 、1840cm -1 、1678cm -1 、1581cm -1 、1512cm -1 、1435cm -1 、864cm -1 、806cm -1 、752cm -1 . Among them, 525cm -1 and 1427cm -1 C 60 The other peaks are basically similar to the IR spectrum of 3,4-bis(5'-bromopentyloxy)benzaldehyde (A).
[0061] (b') Synthesis of N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine (D):
[0062] Under Ar protection, 73.3 mg C 60 (0.102mmol) was dissolved in 72mL of freshly distilled toluene, stirred for 1h, and then 148.5mg (0.517mmol) of B and 32.5mg (0.365mmol) of sarcosine were added, and the mixture was refluxed and stirred at 114°C for 2.5h. After cooling to room temperature, the reaction solution was concentrated. The concentrate was then separated by column chromatography. When the eluent was V 石油醚 :V 乙酸乙酯 =4:1, about 16.3 mg of N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine (D) was isolated, with a yield of about 15.6%.
[0063] like Fig.10 As shown in the figure, δ: 1.29–1.80 (6H, multiple peaks) corresponds to the aliphatic hydrogen in the compound, and 3.43–3.50 (2H, triplet) corresponds to –CH 2 Br hydrogen, 4.06–4.12 (2H, triplet) corresponds to –OCH 2 4.67–4.70 (1H, doublet) correspond to the hydrogen at the 2-position of pyrrolidine, 4.96–5.30 (2H, triplet) correspond to the hydrogen at the 5-position of pyrrolidine, and 2.36 (3H, singlet) corresponds to –CH 3 Hydrogen on the benzene ring (due to C 60 The dispersed conjugation effect causes the two hydrogen atoms to shift to above 7.0, which is exactly the same as CDCl 3 The solvent peak of the graph overlaps), 7.72 (1H, single peak). Due to the low concentration of the compound, the solvent may not be drained, and the solvent peak in the figure is relatively strong. Fig.11 As shown in the infrared spectrum, 524cm -1 、1126cm -1 and 1431cm -1 C 60 The other peaks are basically similar to the infrared spectrum of 3-hydroxy-4-bromopentyloxybenzaldehyde (B).
[0064] Application Example 1: Application of the above fullerene pyrrolidine derivative as a catalyst carrier
[0065] (a) Preparation of Cu nanoparticles supported on N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine)
[0066] (1) Weigh 20 mg of N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or 20 mg of N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine) into a round-bottom flask, add 100 mL of deionized water, and perform ultrasonic treatment at 50°C for 2 h to uniformly disperse N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine) in the deionized water.
[0067] (2) Weigh 20 mg of copper chloride (CuCl 2 ·2H 2 O) was dissolved in 20 mL of deionized water until it was completely dissolved, added to the above round-bottom flask, and placed in an 85°C oil bath with magnetic stirring to allow N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine) and CuCl 2 〃2H 2 OMix evenly.
[0068] (3) Add 5 mL of 1.2 mmol / L ammonia borane (BH) dropwise over 30 min. 3 〃NH 3 ) solution was slowly added to the mixed solution for reduction, and heated in an 80°C oil bath for 3 h under vigorous magnetic stirring. The color of the mixed solution gradually changed from dark green to black, and the solution was then allowed to stand at room temperature for 12 h overnight.
[0069] (4) The mixed solution in the round-bottom flask was transferred to a centrifuge tube and centrifuged for 30 minutes. The centrifuge speed was maintained at 12,000 rpm. After removing the upper deionized water, the mixture was first ultrasonically washed with deionized water for 3 times, and then ultrasonically washed with anhydrous ethanol for 3 times. After each ultrasonic washing, the mixture was centrifuged for 30 minutes to remove the upper solution and retain the lower precipitate. The lower precipitate after centrifugation was dried in a vacuum drying oven at 80° C. for 24 hours to remove moisture, thereby obtaining N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine)-loaded Cu nanoparticle catalyst, the particle size of which was 10-15 nm. The transmission electron microscopy results were as follows: Figure 2 As shown, some particles are agglomerated and the catalyst is stored in a dryer for future use.
[0070] (b) Application of Cu nanoparticles supported on N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine)
[0071] The oxidation of benzyl alcohol is catalyzed by Cu nanoparticle catalyst supported on N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine (or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine), and the specific reaction steps are as follows:
[0072] (1) Add 0.2 mmol of benzyl alcohol, 8 mg of catalyst, and 5 mL of deionized water into the reaction flask, and continue to pass O 2 The reaction bottle was placed in an oil bath, the temperature was raised to 110°C, the reaction was fully reacted for 12 hours, the reaction was stopped, and the product was characterized and analyzed by GC-MS. The chemical reaction equation is as follows: Figure 3 shown.
[0073] (2) The two catalysts were recycled 5 times respectively to investigate their recycling rates. The result data are shown in Table 1.
[0074] Table 1 Conversion rate, selectivity and number of cycles of benzyl alcohol oxidation catalyzed by N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine supported Cu nanoparticles
[0075]
[0076] Table 2 Conversion rate, selectivity and number of cycles of benzyl alcohol oxidation catalyzed by N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine supported Cu nanoparticles
[0077]
[0078]
[0079] As can be seen from Tables 1 and 2, N-methyl-2-[3',4'-di(5"-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine-loaded Cu nanoparticles and N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine-loaded Cu nanoparticles have high catalytic efficiency and good selectivity when catalyzing the oxidation of benzyl alcohol. After the catalyst is recycled for 5 times, its yield can be maintained at more than 93%, and the catalytic activity of the two catalysts is relatively stable. Commonly used oxidation catalysts are homogeneous catalysts, such as salts of precious metals Ru, Rh, Pd, etc., which are not recyclable and have poor product selectivity.
[0080] Obviously, the above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. Use of a fullerene pyrrolidine derivative as a catalyst carrier, It is characterized in that The fullerene pyrrolidine derivative is N-methyl-2-[3',4'-di(5''-bromopentyloxy)phenyl]-3,4-fullerenyl pyrrolidine or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenyl pyrrolidine; the catalyst is N-methyl-2-[3',4'-di(5''-bromopentyloxy)phenyl]-3,4-fullerenyl pyrrolidine-supported Cu nanoparticle catalyst or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenyl pyrrolidine-supported Cu nanoparticle catalyst; Wherein, the preparation method of the fullerene pyrrolidine derivative comprises the following steps: (a) Synthesis of 3,4-di(5'-bromopentyloxy)benzaldehyde or 3-hydroxy-4-bromopentyloxybenzaldehyde; Under inert gas protection, dihydroxybenzaldehyde and Br(CH 2 ) 5 Br, K 2 CO 3 dissolving, heating, stirring and reflux; cooling to room temperature, filtering and concentrating the reaction solution; and then separating the concentrated solution by column chromatography to obtain the intermediate product 3,4-di(5'-bromopentyloxy)benzaldehyde or 3-hydroxy-4-bromopentyloxybenzaldehyde; (b) Synthesis of N-methyl-2-[3',4'-di(5''-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine: Under inert gas protection, 0.01-0.08 molC 60 Dissolve in 20-80 mL toluene solution, stir for 0.5-3 h, add 0.1-0.5 mol of 3,4-di(5'-bromopentyloxy)benzaldehyde and 0.1-0.3 mol of sarcosine, heat to 90-130 °C, reflux and stir for 1-3 h; after cooling to room temperature, concentrate the reaction solution; then separate the concentrated solution by column chromatography to separate N-methyl-2-[3',4'-di(5'-bromopentyloxy)phenyl]-3,4-fullerenepyrrolidine; or, (b') Synthesis of N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine: Under inert gas protection, 0.05-0.25 molC 60 Dissolve in 50-100 mL toluene solution, stir for 0.5-3 h, add 0.2-0.8 mol of 3-hydroxy-4-bromopentyloxybenzaldehyde and 0.2-0.5 mol of sarcosine, heat to 90-130°C, reflux and stir for 1-3 h; after cooling to room temperature, concentrate the reaction solution; then separate the concentrate by column chromatography to separate N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine.
2. The use of a fullerene pyrrolidine derivative as a catalyst carrier according to claim 1, further characterized in that, in the preparation method of the fullerene pyrrolidine derivative, in the column chromatography separation of step (a), the intermediate products 3,4-di(5'-bromopentyloxy)benzaldehyde and 3-hydroxy-4-bromopentyloxybenzaldehyde can be obtained under different eluent conditions; in, When the eluent is V 乙酸乙酯 :V 石油醚 =1:5, 3,4-di(5'-bromopentyloxy)benzaldehyde was separated; when the eluent was V 乙酸乙酯 :V 石油醚 =1:4, 3-hydroxy-4-bromopentyloxybenzaldehyde was separated.
3. The use of a fullerene pyrrolidine derivative as a catalyst carrier as claimed in claim 1, further characterized in that, in the preparation method of the fullerene pyrrolidine derivative, in the column chromatography separation of step (b), when the eluent is pure dichloromethane, N-methyl-2-[3',4'-di(5'-bromopentyloxy)phenyl]-3,4-fullerene pyrrolidine is separated; in the column chromatography separation of step (b'), when the eluent is V 石油醚 :V 乙酸乙酯 =4:1, N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine was isolated.
4. The use as claimed in claim 1, It is characterized in that The catalyst is used for catalytic oxidation of benzyl alcohol.
5. Use of the fullerene pyrrolidine derivative as claimed in claim 1 as a catalyst carrier, It is characterized in that The preparation method of the catalyst is: (1) Add 80-120 mL of deionized water to 30-50 mg of N-methyl-2-[3',4'-di(5''-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine, and perform ultrasonic treatment at 30-70 °C for 1.5-3.5 h to make it uniformly dispersed; (2) Dissolve 10-30 mg of copper chloride in 10-30 mL of deionized water in an oil bath at 60-90°C under magnetic stirring, add the mixture to the above dispersion, and stir to uniformly mix N-methyl-2-[3',4'-di(5''-bromopentyloxy)phenyl]-3,4-fullerenylpyrrolidine or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenylpyrrolidine and copper chloride; (3) Add 1-10 mL of 0.5-2.0 mmol / L ammonia borane (BH 3 ·NH 3 ) solution is slowly added to the above mixed solution for reduction, and heated in a 60-90 ℃ oil bath for 1-5 h under vigorous magnetic stirring, so that the color of the mixed solution gradually changes from dark green to black, and then the solution is allowed to stand at room temperature for 12-24 h; (4) The mixed solution is centrifuged to remove the upper solution, and the lower precipitate after centrifugation is dried to obtain N-methyl-2-[3',4'-di(5''-bromopentyloxy)phenyl]-3,4-fullerenyl pyrrolidine or N-methyl-2-[3'-hydroxy-4'-bromopentyloxyphenyl]-3,4-fullerenyl pyrrolidine-loaded Cu nanoparticle catalyst.
Citation Information
Patent Citations
Synthesis method of fullerene pyrrolidine derivative
CN103396354A
Preparation method of N-methyl-2-(3-methoxyl-4-hydroxyphenyl)-3,4-fulleropyrrolidine
CN107382825A
Method for preparing fullerene nano micron material loaded with transition metal and product of fullerene nano micron material
CN102923690A
Carboxylated sphere carbon metal-organic framework composite material and preparation method and application thereof
CN104475157A
Preparation method and application of fulleropyrrolidine containing 3-methoxyl-4-(5-bromide pentyloxy)phenyl
CN109627204A