A brazing material ring powder for brazing aircraft titanium alloy catheters and a preparation method thereof

By preparing Cu-Zr-Ni titanium alloy powder and forming using thermal isostatic pressing process, the segregation and high porosity problems in the preparation of titanium alloy conduit brazing ring are solved, and the brazing interface strength and performance are improved, satisfying the satisfaction of Use requirements and reduce economic losses.

CN116197572BActive Publication Date: 2024-11-22WUHU STATE-OWNED FACTORY OF MACHINING
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310177589.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-28
Publication Date
2024-11-22
Estimated Expiration
2043-02-28

AI Technical Summary

Technical Problem

The existing titanium alloy conduit brazing ring preparation methods are prone to segregation, metallurgical defects and high porosity, which are difficult to meet the use requirements, resulting in uneven brazing process and economic losses.

Method used

The powder was prepared by aerosolization method and heated by using titanium alloy powders with Cu20%-26%, Zr10%-16%, Ni5%-12%, O≤0.3%, H≤0.3%, Ca≤0.1%. The isostatic pressing process is formed into a dense block, and then mechanically processed into a brazing ring to control the particle size distribution and composition of the powder to ensure high spherical shape and low porosity.

Benefits of technology

It achieves excellent bonding strength and low porosity of the brazing interface, improves the performance of the brazing joint, meets the use requirements and reduces economic losses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116197572B_ABST
    Figure CN116197572B_ABST
Patent Text Reader

Abstract

The invention relates to the field of titanium alloy preparation, in particular to a brazing filler ring powder for brazing of aircraft titanium alloy conduits and a preparation method thereof. The powder comprises the following components: Cu 20%-26%, Zr 10%-16%, Ni 5%-12%, O≤0.3%, H≤0.3%, Ca≤0.1%, and the remainder is titanium element. The specific steps are as follows: S1, material preparation; S2, smelting; S3, atomization; S4, powder collection and screening; S5, preparing the prepared alloy powder into a dense block by adopting a hot isostatic pressing process; S6, machining the prepared dense block into a brazing filler ring by adopting mechanical processing; S7, carrying out a high-frequency induction brazing test on the prepared brazing filler ring and carrying out a performance assessment. The brazing filler ring obtained by the powder is used for high-frequency induction brazing of titanium alloy lubricating oil conduits, ensuring excellent bonding strength of the brazing interface, lower metallurgical defects and reduced porosity, and improving the brazing joint performance, so that the performance after brazing meets the use requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of titanium alloy preparation, in particular to a brazing material ring powder for brazing aircraft titanium alloy conduits and a preparation method thereof. Background Art

[0002] Titanium alloy has high specific strength, specific stiffness, high temperature strength, excellent corrosion resistance and high temperature oxidation resistance. It is widely used in aviation, aerospace, rocket, chemical metallurgy and other fields. At present, aircraft lubricating ducts are made of titanium alloy, and the connection between lubricating oil ducts and pipe joints is made of high-frequency induction brazing. The brazing ring for high-frequency induction brazing is made of titanium-zirconium-copper-nickel alloy. There are currently two methods for preparing this brazing material. One is to prepare titanium-zirconium-copper-nickel brazing material blocks by arc melting in an inert environment, and then machine the blocks into brazing rings for high-frequency induction brazing. The brazing material is easy to produce metallurgical defects and high porosity during the brazing process. Based on the above problems, the total area of ​​pores in the brazing titanium alloy lubricating oil duct is greater than 20% of the brazing seam area, which is difficult to meet the technical requirements, seriously restricts production, and also causes great economic losses. Summary of the invention

[0003] In order to solve the above problems, the present invention provides a brazing filler ring powder for brazing aircraft titanium alloy catheters and a preparation method thereof.

[0004] The invention discloses a brazing filler ring powder for brazing aircraft titanium alloy conduits, the specific components of which are as follows: Cu 20%-26%, Zr 10%-16%, Ni 5%-12%, O≤0.3%, H≤0.3%, Ca≤0.1%, and the balance is titanium element.

[0005] Powder fluidity: ≤20S / 50g, high sphericity ≥0.90.

[0006] Powder particle size distribution: the screening composition is that the powder in the particle size segment ≤45μm accounts for ≤10%, the powder in the particle size segment 45-105μm accounts for ≥80%, and the powder in the particle size segment ≥105μm accounts for ≤10%.

[0007] The melting point of the powder is 880-900℃. When the powder weight is 0.1g, the vacuum degree is 0.01Pa, and the brazing temperature is 920℃, the spreading area is not less than 80mm.2 .

[0008] A method for preparing a brazing material ring powder for brazing an aircraft titanium alloy conduit, the specific steps of which are as follows:

[0009] S1. Prepare materials:

[0010] a. Pre-treat the prefabricated alloy bars for each scheme;

[0011] b. Take samples first to analyze the chemical composition, gas content and impurity content, and proceed to the next step according to the composition ratio;

[0012] c. If the requirements are not met, the raw materials need to be reconfigured until the requirements are met;

[0013] S2, smelting: adjusting the smelting power and smelting frequency of the power supply, smelting the base material prepared in step S1, and obtaining an alloy solution;

[0014] S3, aerosolization:

[0015] a. During the atomization process, the powder quality is controlled by controlling the atomization temperature, atomization pressure, gas flow rate and alloy flow rate and other process parameters;

[0016] b. After atomization, the prepared alloy powder is collected in a powder collecting tank through a cyclone, and the powder collecting tank is directly transferred into the glove box in a sealed state;

[0017] S4. Collecting and sieving powder:

[0018] a. Use a 60-mesh standard sieve for sieving, and the -60-mesh powder is stored in a stainless steel container. The whole process is in an argon protection environment, thus ensuring the cleanliness of the prepared powder;

[0019] b. Collect and sieve the powder, and use 325 mesh and 150 mesh sieves to obtain powder with a particle size of 45-105 μm;

[0020] c. Carry out composition analysis, microstructure analysis and powder performance test on the sieved powder, and finally obtain the powder required by the five schemes;

[0021] S5. Use hot isostatic pressing to prepare the prepared alloy powder into a dense block: the specific hot isostatic pressing process is as follows:

[0022] a. Package preparation:

[0023] The sheath material is 304 stainless steel with a high melting point, and the size and shape of the sheath are designed using CAD software;

[0024] After machining, welding, cleaning and leak detection, a cylindrical package with a thickness of 2mm and a size of Φ15mm×100mm is produced.

[0025] b. Filling powder:

[0026] The powder is filled by selecting the solder powder with the best chemical composition in terms of mechanical and process properties, and then subjected to powder compaction and vacuum pinch-off treatment.

[0027] c. Hot isostatic pressing:

[0028] Hot isostatic pressing of the powder

[0029] d. Take out the dense solder block and test its density;

[0030] S6. Processing the prepared dense block into a brazing ring by mechanical processing:

[0031] Mechanically processing a solder block with a density of ≥99.99% into a solder ring of a required size;

[0032] S7. Carry out high-frequency induction brazing test on the prepared brazing ring and conduct performance assessment.

[0033] The pretreatment in step a of step S1 is specifically degreasing and rust removal.

[0034] The smelting power of step S2 is 30-40KW; the smelting frequency is 2-3KHz.

[0035] The atomization temperature of step S3 is controlled at 800-900° C., the atomization pressure is controlled at 2-4 MPa, the gas flow rate is controlled at 15-18 L / min, and the alloy flow rate is controlled at 0.3-0.8 L / min, and the atomization gas is high-purity argon.

[0036] The technical requirement for the dense block prepared in step S5 is: the density of the prepared dense block is ≥99.99%.

[0037] The specific verification of step S6 is as follows: after the brazing is completed, X-ray flaw detection is carried out to detect whether the brazing seam performance meets the technical requirements for the detection of brazing ring brazing titanium alloy lubricating oil ducts. It is necessary to meet the requirements that the diameter of a single pore in the brazing seam area is less than 0.8 mm, and the total area of ​​the pores does not exceed 12% of the area of ​​the brazing seam area; the area that has not been brazed through in the entire brazing area does not exceed 10% of the area of ​​the brazing area.

[0038] The beneficial effects of the present invention are:

[0039] The brazing ring obtained by the powder of the present invention is used for high-frequency induction brazing of titanium alloy lubricating oil ducts, which ensures excellent bonding strength, lower metallurgical defects and reduced porosity at the brazing interface, and improves the performance of the brazed joint so that the performance after brazing meets the use requirements; the composition of the brazing material is regulated, the mechanical properties of brazing are improved, and a good strength match is achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0041] Figure 1 A schematic diagram of a titanium alloy catheter brazing joint of the present invention;

[0042] Figure 2 Schematic diagram of the solder ring of the present invention Figure 1 ;

[0043] Figure 3 Schematic diagram of the solder ring of the present invention Figure 2 ;

[0044] Figure 4 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION

[0045] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below.

[0046] Embodiment 1:

[0047] like Figures 1 to 4 As shown, a brazing filler ring powder for brazing of aircraft titanium alloy catheters has the following specific components: Cu 20%, Zr 10%, Ni 5%, O ≤ 0.3%, H ≤ 0.3%, Ca ≤ 0.1%, and the balance is titanium element.

[0048] Powder fluidity: ≤20S / 50g, high sphericity ≥0.90.

[0049] Powder particle size distribution: the screening composition is that the powder in the particle size segment ≤45μm accounts for ≤10%, the powder in the particle size segment 45-105μm accounts for ≥80%, and the powder in the particle size segment ≥105μm accounts for ≤10%.

[0050] Technical requirements for mechanical properties of solder:

[0051] The shear strength of TC2 titanium alloy lap joint brazed with brazing filler metal at room temperature is:

[0052] Table 1 Technical requirements for preparation of brazing filler metal

[0053]

[0054] The melting point of the powder is 880-900℃. When the powder weight is 0.1g, the vacuum degree is 0.01Pa, and the brazing temperature is 920℃, the spreading area is not less than 80mm. 2 .

[0055] A method for preparing a brazing material ring powder for brazing an aircraft titanium alloy conduit, the specific steps of which are as follows:

[0056] S1. Prepare materials:

[0057] a. Pre-treat the prefabricated alloy bars for each scheme;

[0058] b. Take samples first to analyze the chemical composition, gas content and impurity content, and proceed to the next step according to the composition ratio;

[0059] c. If the requirements are not met, the raw materials need to be reconfigured until the requirements are met;

[0060] S2, smelting: adjusting the smelting power and smelting frequency of the power supply, smelting the base material prepared in step S1, and obtaining an alloy solution;

[0061] S3, aerosolization:

[0062] a. During the atomization process, the powder quality is controlled by controlling the atomization temperature, atomization pressure, gas flow rate and alloy flow rate and other process parameters;

[0063] b. After atomization, the prepared alloy powder is collected in a powder collecting tank through a cyclone, and the powder collecting tank is directly transferred into the glove box in a sealed state;

[0064] S4. Collecting and sieving powder:

[0065] a. Use a 60-mesh standard sieve for sieving, and the -60-mesh powder is stored in a stainless steel container. The whole process is in an argon protection environment, thus ensuring the cleanliness of the prepared powder;

[0066] b. Collect and sieve the powder, and use 325 mesh and 150 mesh sieves to obtain powder with a particle size of 45-105 μm;

[0067] c. Carry out composition analysis, microstructure analysis and powder performance test on the sieved powder, and finally obtain the powder required by the five schemes;

[0068] S5. Use hot isostatic pressing to prepare the prepared alloy powder into a dense block: the specific hot isostatic pressing process is as follows:

[0069] a. Package preparation:

[0070] The sheath material is 304 stainless steel with a high melting point, and the size and shape of the sheath are designed using CAD software;

[0071] After machining, welding, cleaning and leak detection, a cylindrical package with a thickness of 2mm and a size of Φ15mm×100mm is produced.

[0072] b. Filling powder:

[0073] The powder is filled by selecting the solder powder with the best chemical composition in terms of mechanical and process properties, and then subjected to powder compaction and vacuum pinch-off treatment.

[0074] c. Hot isostatic pressing:

[0075] Using hot isostatic pressing equipment to perform hot isostatic pressing on the loaded powder;

[0076] Hot isostatic pressing process parameters

[0077]

[0078] d. Take out the dense solder block and test its density;

[0079] S6. Processing the prepared dense block into a brazing ring by mechanical processing:

[0080] Mechanically processing a solder block with a density of ≥99.99% into a solder ring of a required size;

[0081] S7. Carry out high-frequency induction brazing test on the prepared brazing ring and conduct performance assessment.

[0082] The pretreatment in step a of step S1 is specifically degreasing and rust removal.

[0083] The smelting power of step S2 is 30-40KW; the smelting frequency is 2-3KHz.

[0084] The atomization temperature of step S3 is controlled at 800-900° C., the atomization pressure is controlled at 2-4 MPa, the gas flow rate is controlled at 15-18 L / min, and the alloy flow rate is controlled at 0.3-0.8 L / min, and the atomization gas is high-purity argon.

[0085] In step S4 c, five composition cases are designed and prepared according to the above alloy powder composition optimization method design and preparation method, which are:

[0086] Scheme 1: Composition: Cu 22%, Zr 10%, Ni 9%, O 0.08%, H 0.05%, Ca 0.05%, the balance is titanium;

[0087] Scheme 2: Composition: Cu 22%, Zr 13%, Ni 9%, O 0.08%, H 0.05%, Ca 0.05%, and the balance is titanium.

[0088] Scheme 3 composition: Cu 22%, Zr 15%, Ni 9%, O 0.05%, H 0.025%, Ca 0.03%, the balance is titanium;

[0089] Scheme 4: composition: Cu 22%, Zr 15%, Ni 10%, O 0.05%, H 0.025%, Ca 0.03%, the balance is titanium;

[0090] Scheme 5: Composition: Cu 25%, Zr 15%, Ni 10%, O 0.05%, H 0.025%, Ca 0.03%, the balance is titanium;

[0091] The powders of the above five components were prepared in turn, and the performance of the prepared solder was evaluated according to the mechanical properties of the solder:

[0092] Brazing material powder performance evaluation table

[0093]

[0094] like Figure 2 and Figure 3 As shown, the technical requirement for the dense block prepared in step S5 is: the density of the prepared dense block is ≥99.99%.

[0095] The specific verification of step S6 is as follows: after the brazing is completed, X-ray flaw detection is carried out to detect whether the brazing seam performance meets the technical requirements for the detection of brazing ring brazing titanium alloy lubricating oil ducts. It is necessary to meet the requirements that the diameter of a single pore in the brazing seam area is less than 0.8 mm, and the total area of ​​the pores does not exceed 12% of the area of ​​the brazing seam area; the area that has not been brazed through in the entire brazing area does not exceed 10% of the area of ​​the brazing area.

[0096] The prepared brazing filler metal ring is used to braze the TC2 titanium alloy lubricating oil pipe. The brazing joint is as follows: Figure 1 In the figure, reference numeral 1 is a titanium alloy conduit, reference numeral 2 is a brazing ring, reference numeral 3 is a titanium alloy sleeve, and L in the figure is the actual overlap amount of brazing penetration. After brazing is completed, X-ray inspection is carried out to detect whether the brazing seam performance meets the technical requirements for the inspection of brazing ring brazing titanium alloy lubricating oil conduits.

[0097] The test results show that the brazing ring in the present invention is specially used for high-frequency induction brazing of titanium alloy lubricating oil ducts, ensuring excellent bonding strength, lower metallurgical defects and reduced porosity at the brazing interface, and improving the performance of the brazed joint, so that its performance after brazing meets the use requirements, and improving the brazing pass rate of titanium alloy lubricating oil ducts, which has high economic benefits.

[0098] Embodiment 1:

[0099] The difference from the first embodiment is that the specific composition of the brazing ring powder for brazing aircraft titanium alloy catheters is as follows: Cu 26%, Zr 16%, Ni 12%, O ≤ 0.3%, H ≤ 0.3%, Ca ≤ 0.1%, and the balance is titanium.

[0100] Embodiment 1:

[0101] The difference from the first embodiment is that the specific composition of the brazing ring powder for brazing aircraft titanium alloy catheters is as follows: Cu 22%, Zr 15%, Ni 9%, O ≤ 0.08%, H ≤ 0.05%, Ca ≤ 0.05%, and the balance is titanium.

[0102] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A brazing ring powder for brazing aircraft titanium alloy catheters, characterized in that: Its specific composition is as follows: Cu20%-26%, Zr10%-16%, Ni5%-12%, O≤0.3%, H≤0.3%, Ca≤0.1%, and the balance is titanium element; powder fluidity: ≤20S / 50g, high sphericity ≥0.90; powder particle size distribution: screening composition ≤45μm particle size segment powder accounts for ≤10%, 45-105μm particle size segment powder accounts for ≥80%, ≥105μm particle size segment powder accounts for ≤10%; the powder melting point is 880-900℃, and when the powder weight is 0.1g, the vacuum degree is 0.01Pa, and the brazing temperature is 920℃, its spreading area is not less than 80mm 2 .

2. A method for preparing a brazing material ring powder for brazing aircraft titanium alloy catheters according to claim 1, characterized in that: The specific steps are as follows: S1. Prepare materials: a. Pre-treat the prefabricated alloy bars for each scheme; b. Take samples first to analyze the chemical composition, gas content and impurity content, and proceed to the next step according to the composition ratio; c. If the requirements are not met, the raw materials need to be reconfigured until the requirements are met; S2, smelting: adjusting the smelting power and smelting frequency of the power supply, smelting the base material prepared in step S1, and obtaining an alloy solution; S3, aerosolization: a. During the atomization process, the powder quality is controlled by controlling the atomization temperature, atomization pressure, gas flow rate and alloy flow rate and other process parameters; b. After atomization, the prepared alloy powder is collected in a powder collecting tank through a cyclone, and the powder collecting tank is directly transferred into the glove box in a sealed state; S4. Collecting and sieving powder: a. Use a 60-mesh standard sieve for sieving, and the -60-mesh powder is stored in a stainless steel container. The whole process is in an argon protection environment, thus ensuring the cleanliness of the prepared powder; b. Collect and sieve the powder, and use 325 mesh and 150 mesh sieves to obtain powder with a particle size of 45-105 μm; c. Carry out composition analysis, microstructure analysis and powder performance test on the sieved powder, and finally obtain the powder required by the five schemes; S5. Use hot isostatic pressing to prepare the prepared alloy powder into a dense block: the specific hot isostatic pressing process is as follows: a. Package preparation: The sheath material is 304 stainless steel with a high melting point, and the size and shape of the sheath are designed using CAD software; After machining, welding, cleaning and leak detection, a cylindrical package with a thickness of 2mm and a diameter of 15mm×100mm is formed; b. Filling powder: The powder is filled by selecting the solder powder with the best chemical composition in terms of mechanical and process properties, and then subjected to powder compaction and vacuum pinch-off treatment. c. Hot isostatic pressing: Hot isostatic pressing of the powder d. Take out the dense solder block and test its density; S6. Processing the prepared dense block into a brazing ring by mechanical processing: Mechanically processing a solder block with a density of ≥99.99% into a solder ring of a required size; S7. Carry out high-frequency induction brazing test on the prepared brazing ring and conduct performance assessment.

3. The method for preparing a brazing ring powder for brazing aircraft titanium alloy catheters according to claim 2, characterized in that: The pretreatment in step a of step S1 is specifically degreasing and rust removal.

4. The method for preparing a brazing ring powder for brazing aircraft titanium alloy catheters according to claim 2, characterized in that: The smelting power of step S2 is 30-40KW; the smelting frequency is 2-3KHz.

5. The method for preparing a brazing filler metal ring powder for brazing aircraft titanium alloy catheters according to claim 2, characterized in that: The atomization temperature of step S3 is controlled at 800-900° C., the atomization pressure is controlled at 2-4 MPa, the gas flow rate is controlled at 15-18 L / min, and the alloy flow rate is controlled at 0.3-0.8 L / min, and the atomization gas is high-purity argon.

6. The method for preparing a brazing filler metal ring powder for brazing aircraft titanium alloy catheters according to claim 2, characterized in that: The technical requirement for the dense block prepared in step S5 is: the density of the prepared dense block is ≥99.99%.

7. The method for preparing a brazing ring powder for brazing aircraft titanium alloy catheters according to claim 2, characterized in that: The specific verification of step S6 is as follows: after the brazing is completed, X-ray flaw detection is carried out to detect whether the brazing seam performance meets the technical requirements for the brazing ring brazing titanium alloy lubricating oil pipe inspection. In the seam area, the diameter of a single pore is less than 0.8 mm, and the total area of ​​the pores does not exceed 12% of the area of ​​the brazing seam; The unpenetrated area in the entire brazing area shall not exceed 10% of the brazing area.

Citation Information

Patent Citations

  • Preparation method for titanium-based amorphous brazing filler metal and application in connection of TC4 titanium alloy and 304 stainless steel

    CN108340093A

  • Brazing filler metal alloy, brazing filler metal, preparing method and application of brazing filler metal alloy and manufactured brazing product

    CN111299901A

  • Design and preparation method of airplane 0Cr14Ni5Mo2Cu steel cone skirt lock damage additive repair powder

    CN114309620A

  • Method for preparing powder of titanium based alloyl solder

    CN1695877A

  • Composite connecting method with transition liquid phase diffusion welding of intermetallic Ti-Al compound alloy

    CN1899747A