A kind of ceramsite produced by resource utilization of fly ash and other solid waste and its preparation method

By combining fly ash with other solid waste and adopting high-temperature roasting technology, the scarcity of resources and process complexity in ceramic production are solved, the high strength and light weight of ceramics are achieved, the standards for light aggregates are met, and the standards for light aggregates are reduced. Pollution risk.

CN116199520BActive Publication Date: 2024-11-08LUOYANG TAIMING ENVIRONMENTAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310258851.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-17
Publication Date
2024-11-08
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

When using fly ash to produce ceramic granules, the prior art faces the problems of resource scarcity and process complexity, and it is difficult to meet the quality requirements of light aggregates, and there is also the risk of secondary pollution.

Method used

By scientifically combining fly ash with other solid waste, such as molybdenum tailings, coal gangue, stone powder, graphite tailings, red mud, dredging silt and slag, adjust the proportion of ceramic granules, and use high-temperature roasting technology to prepare ceramic granules to ensure ceramic granules Particle strength and light weight properties.

Benefits of technology

The high strength and light weight of the ceramic granules are achieved, which avoids the adverse effects of hazardous substances in fly ash on the ceramic granules, reduces process costs and pollution risks, and meets the relevant standards and regulations for light aggregates.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a ceramsite produced by resource utilization of fly ash and other solid wastes and a preparation method thereof, belonging to the technical field of building materials. A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 40-70%, Al2O3: 10-20%, Fe2O3: 3-10%, CaO+MgO: 2-15%, K2O+Na2O: 1.5-10%. Based on the above technical scheme, the present invention makes the various properties of ceramsite products meet the standard requirements of light aggregates on the basis of making full use of hazardous waste fly ash, while improving the strength of ceramsite products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and specifically relates to ceramsite produced by resource utilization of fly ash and other solid wastes and a preparation method thereof. Background Art

[0002] Fly ash is the capture product of the flue gas purification system of municipal solid waste incineration facilities and the bottom ash settled at the bottom of the flue and chimney.

[0003] According to the definition of fly ash, the main source of fly ash is the waste generated by the incineration of domestic waste. The history of waste incineration can be traced back to the mid-to-late 19th century. At that time, it was mainly for public health and safety, and items that may carry viruses such as cholera, typhoid, malaria and other infectious viruses in epidemic areas were burned to control the spread and spread of infectious diseases. In a sense, this is the earliest project to treat solid waste by incineration. The first open furnace was manufactured in the Nottingham market in the UK in 1874. Incineration plants were built in the United States in 1885, Germany in 1896, and France in 1898. Because the technology was primitive and the combustibility ratio was low at that time, the incineration produced a lot of smoke and odor, which seriously polluted the environment. Until the 1960s, waste incineration did not become the main treatment method.

[0004] With the development of technology, large-scale mechanized grates and efficient flue gas purification systems consisting of mechanical dust removal, electrostatic dust removal, washing technology, etc. have appeared in waste incineration in developed countries. Incinerators have also transformed to diversification and automation, and the incineration efficiency and pollution control have been greatly improved.

[0005] At present, the main method of disposing of domestic waste in my country is incineration to generate electricity, and the fly ash produced by incineration is a hazardous waste that is difficult to handle.

[0006] Due to the continuous construction of domestic waste incineration equipment in recent years, the generation of fly ash has been accelerated, which will inevitably cause a large amount of fly ash to accumulate. Solving the fly ash problem is imminent and urgent. A scientific, advanced and thorough measure and method for handling fly ash is urgently needed to protect the environment and prevent secondary pollution caused by waste incineration.

[0007] In the prior art, CN1830885A discloses a ceramsite using fly ash from garbage incineration as raw material and a preparation method thereof, wherein the raw material composition and weight percentage content are: 20% to 80% fly ash and the rest is clay; the ceramsite product is made through batching, granulation and high-temperature calcination; the sintering temperature of the high-temperature calcination is 1000°C to 1400°C.

[0008] CN113387715A discloses a method for preparing fly ash ceramsite with a low sintering temperature. The steps of the fly ash ceramsite preparation method are as follows: 1. Dry and crush the fly ash, diatomaceous earth, soil and composite flux obtained by garbage incineration. 2. Wash the fly ash. 3. Mix the diatomaceous earth with the fly ash and perform a hydrothermal reaction. 4. Mix the fly ash mixture obtained in step 3 with soil and composite flux, roll into granules and sinter at a temperature of 900°C to 1000°C.

[0009] CN111233505A discloses a method for preparing fly ash ceramsite from incineration of garbage. It comprises fly ash from incineration of garbage, Fangzi soil and Jiaobaoshi, wherein the percentage of fly ash from incineration of garbage in roadbed materials is greater than or equal to 30%, the rest is Fangzi soil and Jiaobaoshi, and the percentage of Fangzi soil and Jiaobaoshi in roadbed materials is greater than or equal to 10%. The preparation method comprises crushing, mixing, adding water to each raw material, and then drying and sintering.

[0010] CN113213891A discloses a method for preparing ceramsite using fly ash from garbage incineration and the ceramsite obtained. The invention uses fly ash from garbage incineration as raw material, adds limestone and high silicon material, and adjusts the mass ratio of the main components to: CaO / SiO2=0.2-0.35, (SiO2+Al2O 3) / (CaO+Fe2O3+MgO)=5~8, to control the amount of liquid phase generated during the roasting process, thereby improving the cylinder pressure strength of ceramsite and reducing the roasting temperature. The waste incineration fly ash, limestone, high silicon material and water that meet the above component mass ratio are mixed evenly, after balling and drying, roasted at 800~1200℃ for 5~30min, ceramsite with excellent performance can be obtained.

[0011] The above technical solutions all use traditional raw materials such as clay, diatomaceous earth, ceramsite, pyrophyllite and / or limestone. Some of these raw materials are scarce and difficult to obtain, which significantly limits the treatment of fly ash and the production and application of fly ash ceramsite. In addition, washing the fly ash also increases the difficulty of process treatment and the possibility of secondary pollution.

[0012] In view of this, the present invention is proposed. Summary of the invention

[0013] The technical problem to be solved by the present invention is to provide a ceramsite produced by resource-based utilization of fly ash and other solid wastes, based on the full utilization of hazardous waste fly ash and scientifically match other solid wastes so that the ceramsite products meet the quality requirements of lightweight aggregates and at the same time improve the strength of the ceramsite products.

[0014] Another technical problem to be solved by the present invention is to provide a method for producing ceramsite by resource utilization of fly ash and other solid wastes in view of the deficiencies of the prior art.

[0015] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0016] A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 40-70%, Al2O3: 10-20%, Fe2O3: 3-10%, CaO+MgO: 2-15%, K2O+Na2O: 1.5-10%.

[0017] The effects of the above-mentioned active ingredient of the present invention in ceramsite are as follows:

[0018] SiO2: The main strength material, affecting the temperature of ceramsite expansion, the mass percentage is preferably 40~70%. Too high a content will lead to too high glass phase strength, too high expansion temperature, and poor expansion effect. Too low a content will cause the ceramsite to be unballed and fragile.

[0019] Al2O3: The mass percentage is preferably 10~20%. When fired to a certain temperature, a glass phase is formed. After cooling down, if the aluminum oxide content is too high, the melting temperature of the material will be too high. If the content is too low, the glass phase will be insufficient in strength, and the bubbles will burst the expanded clay, causing the expanded clay to easily break and not form.

[0020] Fe2O3: The main foaming material, which reacts with the reducing substances in the material to generate carbon dioxide, and the mass percentage is preferably 3~10%. If the content is too low, there will be fewer bubbles, and the fired ceramsite will have a large volume, which is not an expanded ceramsite. If the content is too high, the glass phase on the surface of the molten ceramsite will be broken, resulting in the ceramsite not being formed.

[0021] CaO+MgO: Mainly regulate the melting temperature of ceramsite. As the content of these two increases, the melting temperature of the material will decrease. However, if the content of these two components is too high, they will react with heavy metal ions in ceramsite to generate soluble heavy metal water-soluble salts. Therefore, the optimal content range is 2~15%.

[0022] K2O+Na2O: Its main function is similar to that of calcium oxide and magnesium oxide, but the corresponding effect is stronger. The optimal content range is 1.5~10%.

[0023] Furthermore, on the basis of the above-mentioned effective ingredients, the present invention takes the treatment of hazardous waste fly ash as the principle and selects a combination of solid waste and fly ash as raw materials for making expanded clay. The solid waste is preferably a combination of one or more of molybdenum ore tailings, coal gangue, stone powder, graphite tailings, red mud, dredged sludge and slag.

[0024] The physical properties and functions of the raw materials used in the present invention are analyzed as follows:

[0025] Fly ash: Fly ash is the captured material of the flue gas purification system of domestic waste incineration facilities and the bottom ash settled at the bottom of the flue and chimney. The output and quality of fly ash are related to the type of garbage, incineration conditions, type of incinerator and flue gas treatment process. The main heavy metals in fly ash are: lead, copper, cadmium, chromium and zinc. Fly ash contains a large amount of chlorine Cl element, which is mainly accumulated in the fly ash in the form of CaCl2, which helps the formation of glass phase and is beneficial to melt vitrification. The melting point of CaCl2 is only 772℃, and it will volatilize above the melting point. Too much Cl element will cause an increase in the amount of flue gas at high temperature, increasing the load of flue gas treatment. There are large differences in the composition and content of fly ash in different regions. Take the fly ash in Luoyang as an example, its main composition is: SiO2 2.0~6.0%, Al2O3 0.5~2%, Fe2O3 0.1~2.0%, CaO+MgO 40~50%, K2O+Na2O 5~20%, among which the content of CaO+MgO seriously exceeds the content required for ceramsite firing. In addition, the main substances such as Al2O3, Fe2O3 and SiO2 are particularly small, which cannot meet the needs of ceramsite firing.

[0026] Molybdenum tailings: The content of molybdenum in the mine is about 0.1%, and the other components become molybdenum tailings. Molybdenum mines are likened to "mountain movers". Therefore, the stock of molybdenum tailings solid waste is abundant, and it is a relatively easy-to-obtain solid waste material in western Henan. The chemical composition of molybdenum tailings in different regions is different. As an example, molybdenum tailings contain more SiO2, Fe2O3 and CaO. The typical main composition is: SiO2 40~55%, Al2O3 5~6%, Fe2O3 10~20%, CaO+MgO 15~30%, K2O+Na2O 1~2.5%, which is an important material for the formation of ceramsite glass phase and an important skeleton material in the formation process of ceramsite.

[0027] Gangue: Gangue is solid waste discharged during the coal mining and coal washing process. It is a kind of black, gray and hard rock composed of organic and inorganic compounds deposited with coal seams during the coal formation process. The mineral composition of gangue is relatively complex, mainly composed of kaolin, quartz, illite, montmorillonite, limestone, alumina and other substances. Its main components are Al2O3 and SiO2. It also contains varying amounts of Fe2O3, CaO, MgO, Na2O, K2O, SO3 and trace rare elements. The total content of Al2O3, SiO2 and Fe2O3 in gangue is more than 80%. For example, its main components are: SiO2 40~55%, Al2O3 20~30%, Fe2O3 2.0~3.5%, CaO+MgO 0.5~2.0%, K2O+Na2O 1.5~3.0%. Due to the relatively high organic content, its ignition loss is large. The present invention selects coal gangue as fly ash ceramsite material, mainly because it contains a large amount of SiO2 and a very small amount of oxides, which can be beneficial to supplement the skeleton material formed by ceramsite. Moreover, it exists in large quantities in western Henan and is easy to obtain.

[0028] Stone powder: Stone powder is fine solid waste with a particle size of less than 0.16 mm produced during the cutting and polishing process of stone. The main components are carbonate minerals (calcite, dolomite) and granite minerals (quartz, feldspar, amphibole, pyroxene, mica, etc.). Stone powder is mostly precipitate with a high water content. Stone powder contains a large amount of SiO2 and Al2O3 and less oxides. For example, its main composition is: SiO2 60~75%, Al2O3 10~20%, Fe2O3 0.1~1.0%, CaO+MgO 1.0~2.0%, K2O+Na2O 6.0~7.0%; it can be a beneficial supplement to the above materials, is a strong guarantee for the compressive strength of fly ash ceramsite, and can fully make up for the deficiency of skeleton materials.

[0029] Graphite tailings: Graphite tailings are tailings discharged during the graphite mining process. The main mineral components are microcline, quartz, muscovite, and contain a small amount of amphibole, hematite, chlorite and residual graphite from ore dressing. The main components of graphite tailings are SiO2 50~80%, Al2O3 5~20%, and a certain amount of MgO 0.5~10%, Fe2O3 0.1~10.0%, CaO 0.1~5.0%, Na2O 0.1~5%, K2O 1~7%, which are all necessary components for preparing ceramsite; there are some differences in the composition and content of graphite tailings in different regions, but they are still mainly SiO2 and Al2O3, and the content of other components is different. A small amount of other raw materials can be added to adjust the appropriate ceramsite ratio.

[0030] Red mud: Red mud is industrial solid waste discharged when the aluminum industry extracts alumina. Its mineral composition is very complex. The main minerals are aragonite and calcite, followed by opal, gibbsite and goethite. The less abundant ones are titanium minerals, siderite, water glass, sodium aluminate and caustic soda. Among these minerals, aragonite, calcite and siderite play both a skeleton role and a certain cementing role. The main chemical components of red mud are Al2O3, CaO, SiO2, CaO / MgO=15~40%, and Fe2O3 and Na2O, which account for more than 60% of the total red mud. The different bauxite, production process and storage years used in the production of red mud will cause differences in the content of components.

[0031] Dredged sludge: Dredged sludge is a mixture of mud and water produced by dredging sediments in rivers, lakes, estuaries and other water bodies. Its main components are oxides such as SiO2 and Al2O3, with contents ranging from 40~73.6% and 10.1~20.3%. More than 67% of the sludge has an SiO2 content greater than 60%, and also contains a certain amount of oxides such as Na2O, K2O, CaO, MgO, etc.

[0032] Slag: refers to the waste residue (ash) discharged from the combustion of coal or other fuels in industrial and civil boilers and other equipment. Its main chemical components are SiO240~50%, Al2O330~35%, Fe2O34~20%, CaO1~5%. Its mineral composition mainly includes: calcium feldspar, quartz, mullite, magnetite and pyrite, a large amount of silicon-containing glass (Al2O3·2SiO2), and active SiO2, active Al2O3 and a small amount of unburned coal.

[0033] In the present invention, fly ash provides fluxing substances to reduce the firing temperature; molybdenum ore tailings mainly provide materials for forming a glassy phase skeleton; coal gangue and / or red mud and / or slag provide Al2O3 that serves as a skeleton support material and ensures the strength of expanded clay, and beneficially supplements SiO2; stone powder, graphite tailings and / or slag mainly provide SiO2 required for the glassy phase, and beneficially supplement the Al2O3 component to balance the deficiencies of other material components; the fine particles of dredged sludge are conducive to combining with fly ash to roast ultra-light expanded clay.

[0034] A ceramsite produced by resource utilization of fly ash and other solid wastes, which is made of fly ash and solid wastes, wherein the mass percentage of the fly ash is 0.1-30%, and the balance is solid wastes, and the solid wastes are one or a combination of two or more of molybdenum ore tailings, coal gangue, stone powder, graphite tailings, red mud, dredged sludge and slag.

[0035] Preferably, the mass percentage of the fly ash is 10-20%.

[0036] Preferably, the solid waste is a combination of stone powder and at least one of molybdenum ore tailings, coal gangue, graphite tailings, red mud, dredged sludge and slag, which is conducive to the preparation of high-strength lightweight aggregate.

[0037] Preferably, the solid waste is a combination of dredged sludge and at least one of molybdenum mine tailings, coal gangue, stone powder, graphite tailings, red mud and slag, which is conducive to the preparation of ultra-light aggregate.

[0038] The present invention also provides a method for producing ceramsite by resource-recycling fly ash and other solid wastes, which comprises metering and stirring the raw materials, granulating, roasting, cooling, screening and warehousing the finished products.

[0039] As a preferred solution, the metering and mixing is as follows: fly ash and solid waste are provided, and the weight ratio of each raw material is automatically measured with an error of no more than 1%; after measurement, they are respectively conveyed to a high-speed homogenizing device, and fly ash shall not be conveyed exposed; the moisture content of the homogenized material is controlled at 17±3%.

[0040] As a preferred solution, the granulation is carried out by using a pair of rollers, and the diameter is controlled at 10-15 mm.

[0041] As a preferred solution, the roasting is carried out by using a plug-in rotary kiln.

[0042] Further preferably, the calcination process and its parameters include: preheating at 200°C-600°C for 30-40 min; or, preheating at 150°C-400°C for 25-32 min.

[0043] Further preferably, the calcination process and its parameters also include: calcination at 600°C-1100°C for 25-35 min, calcination at 1100°C-1200°C for 12-18 min;

[0044] Alternatively, fire at 400℃~800℃ for 25~35min, and fire at 800℃~1150℃ for 15~20min.

[0045] As a preferred solution, the calcination process and its parameters include: preheating at 200°C to 600°C for 30 to 40 minutes, calcining at 600°C to 1100°C for 25 to 35 minutes, and calcining at 1100°C to 1200°C for 12 to 18 minutes;

[0046] Alternatively, the calcination process and its parameters include: preheating at 150°C-400°C for 25-32 min, sintering at 400°C-800°C for 25-35 min, and sintering at 800°C-1150°C for 15-20 min.

[0047] As a preferred solution, the cooling process is as follows: after the product leaves the kiln, it enters a cooling kiln for cooling, and the cooling time is 20 to 30 minutes.

[0048] As a preferred solution, the screening is as follows: according to the model standard, the products are screened into corresponding models and enter corresponding warehouses.

[0049] As a preferred solution, the finished products are put into storage for inspection and sampling, and then packed into bags.

[0050] The invention also provides application of the fly ash ceramsite in the field of building materials.

[0051] In the National List of Hazardous Wastes, the fly ash category is: HW18 incineration disposal residues, the industry source is: environmental management industry, the waste code is: product of 772-002-18, and the hazardous characteristics are: T (toxicity).

[0052] The harm of fly ash is ultimately harmful to human health. High chlorine content is one of the most obvious characteristics of fly ash in my country, which also brings certain difficulties to its treatment and disposal, because many treatment processes are greatly interfered by chlorine. Acidic substances such as hydrogen chloride produced by the incineration and decomposition of chlorine-containing plastics in domestic waste react with alkaline substances in the flue gas purification system to form products that enter the fly ash, and salt in kitchen waste is also eventually enriched in fly ash. The chlorine content in fly ash is as high as 20% or more, and the chlorine element in fly ash mainly exists in the form of soluble chloride salts, such as sodium chloride, potassium chloride, calcium chloride, etc.

[0053] On the other hand, fly ash has a complex composition. In addition to toxic and harmful substances such as heavy metals and dioxins, it also contains calcium, silicon, aluminum, iron oxides, chloride salts, carbon, sulfur, phosphorus, etc. Moreover, the content of each substance (element) in fly ash will fluctuate greatly with the changes in domestic waste composition, season, incineration conditions, flue gas purification level, etc., which will bring great difficulties to the treatment and disposal of fly ash.

[0054] my country has a large output of fly ash, which is rich in heavy metals and dioxins and has a high volatile chlorine content. Based on the basic properties of fly ash and the main ways to control risks, there are currently two main technical routes for domestic fly ash treatment: landfill disposal and utilization as building materials.

[0055] 1. Landfill disposal: Landfill disposal is to solidify harmful substances by adding chelating agents and then landfill. This technology is relatively mature, with a short process, and can effectively cut off the exposure pathways of pollutants, thereby achieving the goal of minimizing environmental risks. Therefore, landfill has always been the mainstream technical route for fly ash treatment and has been widely recognized and applied. However, there are many disadvantages in landfill disposal, such as occupying a large amount of land resources, the inability to treat harmlessly treated wastewater and waste gas, and the risk of heavy metal and dioxin leaching and many other legacy issues. What's more serious is that because waste incineration plants are relatively scattered and the landfill process is difficult to supervise, there is doubt as to whether waste incineration plants can standardize the addition of chelating agents and landfill in order to control costs. Therefore, landfill disposal is only a stopgap measure.

[0056] 2. Utilization as building materials: Co-treatment in cement kilns: The chemical components contained in fly ash are similar to cement materials. The academic community has begun to explore the use of fly ash to replace cement materials and realize resource utilization. According to relevant experiments, after the fly ash is harmlessly treated, the use of fly ash for the preparation of high-strength concrete can control the amount of heavy metal leakage. Cement and fly ash can be mixed and configured in a certain proportion, and the final mixed mixture can also be used as roadbed filler, which can meet the basic requirements for fillers in the specification. After the implementation of the co-treatment of cement kilns, the processing volume is small, and landfill method is required for co-treatment. In addition, it is difficult to collect and treat wastewater and waste gas in a harmless manner. In addition, fly ash has a particularly large impact on the performance of cement, and the control of the amount of fly ash input needs to be very precise, which cannot be met by the existing cement production process. At the same time, there is also a risk of leaching heavy metals and dioxins. Buildings constructed with fly ash cement will inevitably have complex and heavy construction waste treatment after their service life expires.

[0057] Sintering and melting: The existing sintering technology is to mix washed fly ash with other corresponding materials and sinter it at high temperature to form lightweight aggregate for construction. Sintering has similar advantages as cement kiln co-treatment. However, since the amount of sintering flue gas is relatively small, if heavy metals are "intentionally" driven into the flue gas during the sintering process and then recovered or treated, the transfer or dilution of heavy metals can be avoided.

[0058] Melting is the process of melting the fly ash at a higher temperature than sintering and then solidifying it into a glassy body. Most of the heavy metals are volatilized into the flue gas and then captured, and a small part is fixed in the glassy mineral structure. However, the problems are that the process equipment is complex, the energy consumption is high, and the cost is high.

[0059] As a lightweight aggregate, ceramsite has excellent multifunctional characteristics such as low density, high cylinder pressure strength, high porosity, thermal insulation, corrosion resistance, good seismic resistance and frost resistance, and resistance to alkali aggregate reaction. Its remarkable characteristics are formed by the internal honeycomb multi-closed-cell structure and the external glaze wrapping. During high-temperature firing, a variety of substances react chemically to generate some gas. The material melts at high temperature under the action of the flux component to hinder the expansion of the gas and form a uniform closed pore system. At present, there are two main types of substances for firing expansion. One is the expansion caused by the generation of bubbles by Fe2O3 and other oxides at high temperature; the other is the expansion of inorganic carbon-based materials in the proportioning material.

[0060] The main characteristics of expanded clay determine its properties. Both the drying stage and the roasting stage are closely related to the formation of pores. The control of each stage requires repeated tests and adjustments to make the finished expanded clay have better performance and higher output.

[0061] In the preparation of the ceramsite of the present invention, the overall temperature control is mainly divided into the following stages: 1. Preheating stage, the water content of the ceramsite body evaporates and the organic matter decomposes; 2. Firing stage, bubbles are generated and a liquid phase is formed, and the presence of the liquid phase helps to melt and solidify the heavy metal elements in the fly ash of garbage incineration; 3. Cooling stage, mainly controlling the heat of the ceramsite body subjected to heat radiation and heat conduction in the kiln, and sintering a qualified finished product.

[0062] Specifically, the preheating stage is a slow heating, the main purpose of which is to remove moisture, prevent the green body from bursting, and ensure the integrity of the body; after the preheating stage, it enters the firing stage, the temperature rises rapidly and the heat is evenly distributed, which is beneficial to the expansion of the material; as the temperature continues to rise, a large amount of gas overflows to form pressure, which causes the body to expand and form uniform closed-cell bubbles. The temperature needs to be strictly controlled in this stage, because the temperature zone for foaming into balls is narrow, which is prone to bonding or clamping; after the roasting stage, it enters the cooling stage, and the product is cooled to room temperature (25±5℃).

[0063] In the present invention, the sintering temperature of fly ash ceramsite is 1100-1200°C, and the residence time is appropriate, at which time the dioxins will be completely decomposed; in the cooling stage, when the temperature drops to 300-500°C, the chloride ions and other components in the flue gas will resynthesize dioxins and enter the flue gas, which can be discharged into the air after conventional purification.

[0064] The present invention has been tested in large quantities and has produced qualified products by adopting the above-mentioned manufacturing process, which has proved that the material ratio is reasonable and the baking temperature control range is appropriate.

[0065] Compared with the prior art, the present invention has the following beneficial effects:

[0066] The present invention uses hazardous waste fly ash as raw material, matches it with suitable solid waste, and produces ceramsite products through a firing process. On the basis of fully utilizing the fly ash, the ceramsite products meet the relevant standard regulations of lightweight aggregates, and effectively avoid the adverse effects of harmful substances in the fly ash on the ceramsite products.

[0067] Compared with chelating solidification landfill treatment, the present invention avoids the potential pollution hazards of harmful substances such as wastewater and waste gas generated after landfill treatment and the occupation of a large amount of land resources; compared with the method of co-disposing fly ash in cement kilns, it does not require a water washing process, has low investment cost, no secondary pollution, and stable product quality; the present invention also innovates in raw materials, which is completely different from traditional sintering that uses clay and shale as raw materials, and can fully utilize fly ash and other solid wastes; the product ceramsite of the present invention is widely used and can be made into self-insulating blocks, lightweight aggregate concrete, prefabricated building components, thermal insulation materials, filter materials, cultural stones, sound insulation boards, etc.

[0068] Generally, the soluble chlorine content in fly ash is 18-25wt%. The soluble chlorine content in the ceramsite prepared by using the fly ash in the present invention is less than 2wt%, which complies with the provisions of HJ1134 "Technical Specifications for Pollution Control of Fly Ash from Incineration of Domestic Waste"; the chloride content (calculated by the mass of chloride ions) is less than 0.02wt%, which complies with the provisions of GB / T17431.1 "Light Aggregate and Its Test Method Part 1: Light Aggregate".

[0069] The fly ash ceramsite prepared by the present invention is rich in resources and can be prepared by easily obtaining materials, achieving the goal of "hazardous waste + solid waste = new green building materials". All indicators meet the requirements of "Light Aggregate and Experimental Methods Thereof Part I: Light Aggregate" GB / T17431.1-2010, and can be used to prepare light aggregate or high-strength light aggregate of different density levels of 300-800kg / m³, and cylinder pressure strength, water absorption rate, softening coefficient, boiling mass loss, ignition loss, sulfide and sulfate content, chloride content (measured in chloride ions) and radioactivity all meet the requirements of standards; compared with existing fly ash ceramsite, the strength is more significant at the same density level. DETAILED DESCRIPTION

[0070] In order to better understand the present invention, the content of the present invention is further clearly set forth in conjunction with the embodiments below, but the protection content of the present invention is not limited to the following embodiments. In the following description, a large number of specific details are provided in order to provide a more thorough understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can be implemented without one or more of these details.

[0071] In the present invention, the fly ash ceramsite is made of fly ash and solid waste, the mass percentage of fly ash is 0.1-30%, and the balance is solid waste, and the solid waste is one or a combination of more than two of molybdenum ore tailings, coal gangue, stone powder, graphite tailings, red mud, dredged sludge and slag.

[0072] As a preferred solution, the mass percentage of fly ash is selected to be 10-20%, and the remainder is solid waste.

[0073] For solid waste, you can choose: a combination of molybdenum tailings, coal gangue and stone powder, and the mass percentage of molybdenum tailings, coal gangue and stone powder in the solid waste can be selected from 0.1% to 99.9%;

[0074] or a combination of molybdenum tailings, coal gangue, stone powder and slag, and the mass percentage of the molybdenum tailings, coal gangue, stone powder and slag in the solid waste can be selected as any value of 0.1-99.9%%;

[0075] or a combination of stone powder and dredged sludge, and the mass percentage of the stone powder and dredged sludge in the solid waste can be selected from 0.1% to 99.9%;

[0076] Or a combination of slag, stone powder and red mud, and the mass percentage of slag, stone powder and red mud in the solid waste can be selected as any value of 0.1~99.9%.

[0077] In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limiting. Therefore, other examples of the exemplary embodiments may have different values.

[0078] Example 1

[0079] A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 50.03%, Al2O3: 16.39%, Fe2O3: 3.57%, CaO+MgO: 9.73%, K2O+Na2O: 4.77%;

[0080] The above-mentioned method for resource-based utilization of fly ash and other solid waste to produce ceramsite includes metering and mixing the raw materials, granulating, roasting, cooling, screening and warehousing the finished products, wherein:

[0081] Metering and mixing: provide 10 parts by weight of fly ash, 20 parts by weight of molybdenum ore tailings, 40 parts by weight of coal gangue and 30 parts by weight of stone powder, and automatically measure according to the weight ratio of each raw material, with an error of no more than 1%; after measurement, they are respectively conveyed to the high-speed homogenizing device, and fly ash shall not be conveyed naked; the moisture content of the homogenized material is controlled at 17±3%;

[0082] Granulation: Double roller granulation is adopted, and the diameter is controlled at 10~15mm;

[0083] Calcination: The plug-in rotary kiln is used for calcination. The process and parameters include: preheating and drying at 200°C for 40 minutes; calcination at 600°C for 30 minutes; and further calcination at 1100°C for 15 minutes.

[0084] Cooling: After leaving the kiln, the product enters the cooling kiln for cooling, and the cooling time is 23 minutes;

[0085] Screening: According to the model standards, the products are screened into corresponding models and sent to the corresponding warehouse.

[0086] Finished product storage: inspect and keep samples, then pack into bags and store.

[0087] Example 2

[0088] A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 48.29%, Al2O3: 19.03%, Fe2O3: 3.07%, CaO+MgO: 9.09%, K2O+Na2O: 5.72%,

[0089] The raw material composition is: 15 parts by weight of fly ash, 10 parts by weight of molybdenum ore tailings, 40 parts by weight of coal gangue, 30 parts by weight of stone powder and 5 parts by weight of slag.

[0090] The preparation method thereof is different from that of Example 1 in that the calcination process and its parameters include: preheating and drying at 300°C for 38 minutes; calcining at 700°C for 32 minutes; and further calcining at 1100°C for 18 minutes.

[0091] Example 3

[0092] A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 44.62%, Al2O3: 12.01%, Fe2O3: 9.89%, CaO+MgO: 12.59%, K2O+Na2O: 7.92%,

[0093] The raw material composition is: 20 parts by weight of fly ash, 10 parts by weight of stone powder and 70 parts by weight of dredged sludge.

[0094] The difference from the preparation method in Example 1 is that the roasting process and its parameters include: preheating and drying at 400°C for 35 minutes; firing at 850°C for 30 minutes; and continuing firing at 1130°C for 15 minutes.

[0095] Example 4

[0096] A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 40.23%, Al2O3: 15.13%, Fe2O3: 3.02%, CaO+MgO: 14.96%, K2O+Na2O: 8.81%,

[0097] The raw material composition is: 30 parts by weight of fly ash, 35 parts by weight of coal gangue, 20 parts by weight of stone powder, 5 parts by weight of graphite tailings and 10 parts by weight of dredged sludge.

[0098] The preparation method thereof is different from that of Example 1 in that the calcination process and its parameters include: preheating and drying at 500°C for 32 minutes; calcining at 930°C for 30 minutes; and further calcining at 1150°C for 15 minutes.

[0099] Example 5

[0100] A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 60.92%, Al2O3: 14.09%, Fe2O3: 4.15%, CaO+MgO: 4.64%, K2O+Na2O: 6.07%,

[0101] The raw material composition is: 5 parts by weight of fly ash, 5 parts by weight of molybdenum ore tailings, 75 parts by weight of stone powder, 10 parts by weight of graphite tailings and 5 parts by weight of red mud.

[0102] The preparation method thereof is different from that of Example 1 in that the calcination process and its parameters include: preheating and drying at 600°C for 30 minutes; calcining at 1000°C for 27 minutes; and further calcining at 1170°C for 13 minutes.

[0103] Example 6

[0104] A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 45.05%, Al2O3: 11.53%, Fe2O3: 6.92%, CaO+MgO: 14.65%, K2O+Na2O: 5.73%,

[0105] The raw material composition is: 12 parts by weight of fly ash, 30 parts by weight of molybdenum ore tailings, 10 parts by weight of slag, 3 parts by weight of graphite tailings, and 45 parts by weight of dredged sludge;

[0106] The preparation method thereof is different from that of Example 1 in that the calcination process and its parameters include: preheating and drying at 600°C for 35 minutes; calcining at 1100°C for 25 minutes; and further calcining at 1200°C for 15 minutes.

[0107] Example 7

[0108] A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 40.12%, Al2O3: 13.07%, Fe2O3: 7.23%, CaO+MgO: 12.90%, K2O+Na2O: 9.83%,

[0109] The raw material composition is: 25 parts by weight of fly ash and 75 parts by weight of dredged sludge;

[0110] The preparation method thereof is different from that of Example 2 in that the calcination process and its parameters include: preheating and drying at 150°C for 32 minutes; calcining at 400°C for 35 minutes; and continuing calcining at 800°C for 20 minutes.

[0111] Example 8

[0112] A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 67.50%, Al2O3: 10.12%, Fe2O3: 3.41%, CaO+MgO: 2.97%, K2O+Na2O: 1.71%,

[0113] The raw material composition is: 30 parts by weight of fly ash, 10 parts by weight of coal gangue, 40 parts by weight of stone powder, and 20 parts by weight of graphite tailings;

[0114] The preparation method thereof is different from that of Example 3 in that the calcination process and its parameters include: preheating and drying at 160°C for 30 minutes; calcining at 500°C for 32 minutes; and further calcining at 900°C for 18 minutes.

[0115] Example 9

[0116] A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 57.23%, Al2O3: 12.35%, Fe2O3: 9.01%, CaO+MgO: 8.24%, K2O+Na2O: 3.01%,

[0117] The raw material composition is: 25 parts by weight of fly ash, 35 parts by weight of stone powder, 10 parts by weight of red mud, and 30 parts by weight of dredged sludge;

[0118] The preparation method thereof is different from that of Example 4 in that the calcination process and its parameters include: preheating and drying at 300°C for 27 minutes; calcining at 650°C for 30 minutes; and continuing calcining at 1000°C for 16 minutes.

[0119] Example 10

[0120] A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the effective components and their mass percentages are as follows: SiO2: 59.71%, Al2O3: 11.03%, Fe2O3: 5.11%, CaO+MgO: 4.07%, K2O+Na2O: 3.84%,

[0121] The raw material composition is: 20 parts by weight of fly ash, 10 parts by weight of molybdenum ore tailings, 20 parts by weight of slag, 20 parts by weight of graphite tailings, and 30 parts by weight of dredged sludge;

[0122] The preparation method thereof is different from that of Example 5 in that the calcination process and its parameters include: preheating and drying at 400°C for 25 minutes; calcining at 800°C for 25 minutes; and further calcining at 1150°C for 15 minutes.

[0123] The following is a comparative case description.

[0124] Comparative Example 1

[0125] A ceramsite produced by resource utilization of fly ash and other solid wastes, using fly ash as raw material, wherein the effective components and their mass percentages are as follows: SiO2: 4.52%, Al2O3: 1.02%, Fe2O3: 0.72%, CaO+MgO: 45.21%, K2O+Na2O: 17.4%; the preparation method is the same as that in Example 1.

[0126] The test found that fly ash alone cannot be used to prepare shaped expanded clay, so relevant indicators cannot be tested.

[0127] Comparative Example 2

[0128] A ceramsite produced by resource utilization of fly ash and other solid wastes, which is different from Example 1 in that the effective ingredients and their mass percentages are: SiO2: 35.2%, Al2O3: 15.21%, Fe2O3: 5.31%, CaO+MgO: 25.24%, K2O+Na2O: 3.45%; the preparation method is the same as that of Example 1.

[0129] Comparative Example 3

[0130] A ceramsite produced by resource utilization of fly ash and other solid wastes, which is different from Example 2 in that the roasting process steps and parameters are fired at 1200° C. for 15 minutes.

[0131] Comparative Example 4

[0132] A ceramsite produced by resource utilization of fly ash and other solid wastes, which is different from Example 2 in that: the roasting process steps and parameters are preheating and drying at 500°C for 30 minutes; heating to 1100°C and continuing to fire for 30 minutes.

[0133] Next, the contents of the evaluation test will be described.

[0134] The test items, index requirements and reference standards are shown in the following table:

[0135] .

[0136] The fly ash ceramsite prepared in the above Examples 1 to 4 and Comparative Examples 2 to 4 was tested according to the regulations, and the results were averaged. The test results are shown in the following table:

[0137] .

[0138] The above results show that the various indicators of the fly ash ceramsite prepared by the present invention meet the relevant provisions of "Light Aggregate and Its Test Method Part 1: Light Aggregate" GB / T17431.1-2010, and light aggregates of different density grades can be prepared. At the same density grade, the cylinder compression strength of the ceramsite of the present invention can meet the requirements of high-strength light aggregate, showing significant progress.

[0139] Comparative Example 2 Compared with Example 1, the SiO2 content is reduced, the CaO+MgO content is increased, and the ceramsite product prepared has a high 3 At the graded density, the cylinder pressure strength does not meet the index requirements of high-strength lightweight aggregate, that is, the cylinder pressure strength is less than 5.0, and the softening coefficient and boiling mass loss rate are reduced. The cylinder pressure strength of the ceramsite product prepared according to Comparative Example 3 also does not meet the requirements of 800kg / m 3 The index requirements of high-strength lightweight aggregate under grade density, water absorption rate, softening coefficient, and boiling mass loss rate are significantly deteriorated. The ceramsite product prepared according to Comparative Example 4 has improved various indicators compared with Comparative Example 3, but is still significantly different from Example 2 overall, and the cylinder pressure strength does not meet 800kg / m 3 Index requirements for high-strength lightweight aggregates at graded density.

[0140] It can be seen from this that the effective ingredients of the fly ash ceramsite of the present invention are scientifically and reasonably matched, and the matching of the preparation process and the ingredients is good, and finally a ceramsite product with superior performance is obtained, especially the ability to synergistically improve the strength of the ceramsite.

[0141] The ceramsite product prepared by the invention can be used as light aggregate or high-strength light aggregate to make self-insulating blocks, light aggregate concrete, assembled building components, thermal insulation materials, filter materials, cultural stones, sound insulation boards, etc., and has a wide range of uses.

[0142] In addition, those skilled in the art should understand that, although there are many problems in the prior art, each embodiment or technical solution of the present invention can be improved in only one or several aspects, without having to solve all the technical problems listed in the prior art or background technology at the same time. Those skilled in the art should understand that the content not mentioned in a claim should not be used as a limitation on the claim.

[0143] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

Claims

1. A ceramsite produced by resource utilization of fly ash and other solid wastes, wherein the density of the ceramsite is 300-370 kg / m³, characterized in that: It is made of fly ash and solid waste, the mass percentage of the fly ash is 0.1-30%, and the balance is solid waste; the solid waste is a combination of two or more of molybdenum tailings, coal gangue, stone powder, graphite tailings, red mud, dredged sludge and slag; the effective components of the ceramsite and their mass percentages are as follows: SiO2: 40.23-60.92%, Al2O3: 10-16.39%, Fe2O3: 3-5.11%, CaO+MgO: 8.24-15%, K2O+Na2O: 5.72-10%, The production method of ceramsite comprises: providing fly ash and solid waste, automatically measuring according to the weight ratio of each raw material, with an error of no more than 1%, and respectively transmitting them to a high-speed homogenizing device after measuring, wherein the fly ash shall not be transmitted exposed, and the moisture content of the homogenized material is controlled at 17±3%; adopting double-roller granulation, with the diameter controlled at 10-15 mm; adopting a plug-in rotary kiln for roasting, wherein the roasting process and its parameters comprise: preheating at 150-400°C for 25-32 min, firing at 400-800°C for 25-35 min, and firing at 800-1150°C for 15-20 min; after the product leaves the kiln, entering a cooling kiln for cooling, and the cooling time is 20-30 min; screening the product into corresponding models according to the model standard, and putting the finished product into storage.

2. The ceramsite produced by resource utilization of fly ash and other solid wastes as claimed in claim 1, characterized in that: The mass percentage of the fly ash is 10-20%.

3. The ceramsite produced by resource utilization of fly ash and other solid wastes as claimed in claim 2, characterized in that: The solid waste is a combination of rock powder and at least one of molybdenum ore tailings, coal gangue, graphite tailings, red mud, dredged sludge and slag.

4. The ceramsite produced by resource utilization of fly ash and other solid wastes as claimed in claim 1, characterized in that: The solid waste is a combination of dredged sludge and at least one of molybdenum mine tailings, coal gangue, stone powder, graphite tailings, red mud and slag.

5. Application of ceramsite produced by resource utilization of fly ash and other solid wastes as claimed in any one of claims 1 to 4 in building materials.