Lubricating oil, preparation method and use thereof

By oxidizing the black phosphorus nanosheets, combining fatty acids and base oils, a super-sliding interface of phosphorus oxides and amorphous carbon is formed, which solves the problem of friction and wear of mechanical equipment, realizes ultra-sliding at the macroscopic scale, and reduces energy loss and wear of parts.

CN116200220BActive Publication Date: 2024-11-26TSINGHUA UNIVERSITY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211605669.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-14
Publication Date
2024-11-26
Estimated Expiration
2042-12-14

AI Technical Summary

Technical Problem

Friction and wear of machinery during operation leads to energy consumption, component damage and environmental pollution, and existing liquid lubricants lack load capacity under high contact pressures, limiting their industrial applications.

Method used

Black phosphorus nanosheets, oxidizing solutions and fatty acids are used to oxidize under vacuum to form a superslip interface between phosphorus oxide and amorphous carbon, reduce the friction coefficient and achieve superslip at the macroscopic scale.

Benefits of technology

It significantly reduces the friction coefficient, achieves ultra-slip on the macroscopic scale in atmospheric environment, reduces energy loss and wear, and improves the life and safety of mechanical equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116200220B_ABST
    Figure CN116200220B_ABST
Patent Text Reader

Abstract

The present application relates to a lubricating oil, a preparation method and use thereof, and belongs to the technical field of lubricating materials. The preparation method of the lubricating oil provided in the present application comprises the following steps: S1. Mixing black phosphorus nanosheets, a solvent and an oxidizing solution to perform a primary oxidation treatment on the black phosphorus nanosheets to obtain a dispersion; S2. Mixing the dispersion, fatty acid and base oil and drying them under a vacuum environment to perform a secondary oxidation treatment on the black phosphorus nanosheets and remove the solvent; S3. Separating the lubricating oil from the mixed solution obtained in step S2. The lubricating oil obtained by this preparation method can reduce the friction coefficient and achieve macroscopic super-lubricity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lubricating materials, and in particular to a lubricating oil, a preparation method thereof and uses thereof. Background Art

[0002] Mechanical equipment does not require friction and wear in many occasions, such as the friction between automobile engines, gears and shafts, which not only causes energy consumption and component wear and failure, but also causes serious pollution to the environment. Wear is one of the main forms of damage to mechanical parts, and the failure caused by wear is also uncertain and hidden, posing a serious safety hazard. Therefore, finding new materials and new methods to reduce friction and wear to a negligible level has long been the focus of researchers, which is of great significance for saving energy and resources, extending equipment life, improving mechanical safety, and reducing environmental pollution. Summary of the invention

[0003] Based on this, it is necessary to provide a lubricating oil that can reduce the friction coefficient and achieve macroscopic super-lubricity, and a preparation method and use thereof.

[0004] The first aspect of the present application provides a method for preparing a lubricating oil, comprising the following steps:

[0005] S1. mixing black phosphorus nanosheets, a solvent and an oxidizing solution to perform a primary oxidation treatment on the black phosphorus nanosheets to obtain a dispersion;

[0006] S2. mixing the dispersion, fatty acid and base oil and drying them under vacuum to perform secondary oxidation on the black phosphorus nanosheets and remove the solvent;

[0007] S3. Separating lubricating oil from the mixed liquid obtained in step S2.

[0008] In some embodiments, the fatty acid includes one or more of oleic acid, stearic acid, ricinoleic acid, and elaidic acid.

[0009] In some embodiments, the solvent comprises anhydrous ethanol.

[0010] In some embodiments, the oxidizing solution comprises a hydrogen peroxide solution.

[0011] In some more specific embodiments, the mass fraction of the hydrogen peroxide solution is 15% to 30%.

[0012] In some embodiments, the base oil comprises a polyalphaolefin.

[0013] In some more specific embodiments, the polyalphaolefin includes one or more of PAO2, PAO4, PAO6, and PAO10.

[0014] In some embodiments, the mass ratio of the black phosphorus nanosheets to the solvent is 1:(50-200).

[0015] In some embodiments, the volume ratio of the mixture formed by dispersing the black phosphorus nanosheets in the solvent to the oxidizing solution is (20-100):1.

[0016] In some embodiments, the volume ratio of the dispersion, the fatty acid and the base oil is 1:(1-10):(1-50).

[0017] In some embodiments, the process of mixing the black phosphorus nanosheets, the solvent and the oxidizing solution in step S1 includes: mixing the black phosphorus nanosheets with the solvent, performing a first stirring, and then mixing with the oxidizing solution, and performing a second stirring.

[0018] In some more specific embodiments, the first stirring time is 30 min to 50 min.

[0019] In some more specific embodiments, the second stirring time is 10 min to 60 min.

[0020] In some more specific embodiments, both the first stirring and the second stirring are magnetic stirring.

[0021] In some embodiments, the process conditions of step S2 include: the mixing and stirring time is 15 min to 30 min, the temperature of the vacuum environment is 80° C. to 100° C., the vacuum degree is -0.06 MPa to -0.08 MPa, and the drying time is 20 min to 60 min.

[0022] In some embodiments, step S3 comprises: magnetically stirring the mixed solution obtained in step S2 for 30 min to 60 min, and taking an upper oil sample after centrifugation to obtain lubricating oil.

[0023] The second aspect of the present application provides a lubricating oil, which is prepared by the preparation method described in the first aspect of the present application.

[0024] The third aspect of the present application provides a use of a lubricating oil prepared by the preparation method described in the first aspect of the present application or the lubricating oil described in the second aspect of the present application in the preparation of a lubricating product.

[0025] Compared with conventional technologies, the above lubricating oil, its preparation method and use have at least the following advantages:

[0026] In the above-mentioned method for preparing lubricating oil, phosphorus oxide is formed on the surface or near the surface of black phosphorus nanosheets after oxidation, and is used in combination with fatty acids and base oil. The formed lubricating oil contains oxidized black phosphorus and can achieve decomposition and carbonization of fatty acids at the interface of oxidized black phosphorus during the friction process, thereby constructing a layer of super-slippery interface formed by phosphorus oxide and amorphous carbon, thereby reducing the friction coefficient and achieving super-slippery at a macroscopic scale. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a graph of the friction coefficient of the lubricating oil prepared in Example 1 of the present application under a load of 1N.

[0028] Figure 2 This is a graph of the friction coefficient of the lubricating oil prepared in Example 2 of the present application under a load of 1N.

[0029] Figure 3 This is a graph of the friction coefficient of the lubricating oil prepared in Comparative Example 1 of the present application under a load of 1N. DETAILED DESCRIPTION

[0030] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0031] In the description of this application, unless otherwise defined, unspecified professional terms and professional words have the same meaning as those commonly understood by those skilled in the art and are common knowledge of those skilled in the art, and unspecified methods are conventional methods known to those skilled in the art. The term "multiple" in this application means at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0032] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0033] Superlubricity is a phenomenon used to describe the almost complete disappearance of friction between two surfaces in relative motion. It is generally accepted that lubrication conditions with a friction coefficient of less than 0.01 are classified as superlubricity. Superlubricity not only means an order of magnitude reduction in the friction coefficient, but also means that the wear caused by the reduction of several orders of magnitude in the friction coefficient is almost negligible. In this case, if superlubricity can be achieved at the macro level, it will greatly reduce energy loss and increase the life of mechanical equipment.

[0034] At present, superlubricity is divided into two categories according to the contact form of the friction pair: solid superlubricity (solid-solid contact) and liquid superlubricity (solid-liquid-solid contact). Solid superlubricity usually has strict structural requirements on the friction pair (such as non-commensurate contact) and requires special environmental conditions (such as ultra-high vacuum, etc.). In contrast, liquid superlubricity can be achieved in macroscopic and atmospheric environments. At present, liquid superlubricity can be achieved through a variety of liquid lubricants, such as phosphoric acid aqueous solution, glycerol / acid mixed aqueous solution, polyethylene glycol / boric acid aqueous solution, ionic liquid aqueous solution, etc. The use of low-viscosity liquids is the main way to achieve liquid superlubricity, but due to the weak carrying capacity of low-viscosity liquids, the contact pressure during liquid superlubricity is mostly lower than the contact pressure of solid superlubricity, which greatly limits the industrial application of liquid superlubricity.

[0035] Black phosphorus is a new type of two-dimensional material with excellent properties in heat, force, light, electricity, etc. At the same time, as a new type of lubricating additive, it also shows great application potential in the field of tribology. In recent years, black phosphorus has made breakthroughs in the field of water-based superlubricity, and can achieve macroscopic superlubricity under extreme pressures of up to 1.2GPa. However, due to the limitations of the applicability of water-based superlubricity, how to achieve macroscopic superlubricity of black phosphorus in an oil-based environment and then realize its engineering application remains a challenge. In view of this, the present application provides a lubricating oil, its preparation method and use.

[0036] An embodiment of the present application provides a method for preparing lubricating oil, comprising the following steps:

[0037] S1. mixing black phosphorus nanosheets, a solvent and an oxidizing solution to perform a primary oxidation treatment on the black phosphorus nanosheets to obtain a dispersion;

[0038] S2. mixing the dispersion, fatty acid and base oil and drying them under vacuum to perform secondary oxidation on the black phosphorus nanosheets and remove the solvent;

[0039] S3. Separating lubricating oil from the mixed liquid obtained in step S2.

[0040] The solvent in the above preparation method is used to disperse the black phosphorus nanosheets, so that the black phosphorus nanosheets and the oxidizing solution are fully oxidized to form phosphorus oxides on the surface or near the surface of the black phosphorus nanosheets, that is, oxidized black phosphorus; when the dispersion, fatty acid and base oil are mixed and dried under a vacuum environment in step S2, since the oxidizing solute in the oxidizing solution still remains in the dispersion, the oxidizing solute and the black phosphorus nanosheets can undergo oxidation reaction again to form phosphorus oxides. On the one hand, the friction performance of the phosphorus oxides formed on the surface or near the surface of black phosphorus is relatively excellent. On the other hand, phosphorus oxides are easy to form some hydrogen bonds with fatty acids during the friction process. These hydrogen bonds are conducive to the adsorption of phosphorus oxides, and then conducive to phosphorus oxides entering the friction interface of the friction process, so that fatty acids are decomposed and carbonized at the oxidized black phosphorus interface. The above preparation method actively oxidizes the black phosphorus nanosheets, and then adds fatty acids as an organic carbon source and combines with base oil. The lubricating oil formed contains oxidized black phosphorus and realizes the decomposition and carbonization of fatty acids at the oxidized black phosphorus interface during the friction process, and finally constructs a layer of super-slip interface formed by phosphorus oxides and amorphous carbon, reduces the friction coefficient, and achieves super-slip at a macroscopic scale.

[0041] In some embodiments, the fatty acid includes one or more of oleic acid, stearic acid, ricinoleic acid, and elaidic acid.

[0042] In some embodiments, the solvent includes anhydrous ethanol. It should be noted that since the black phosphorus nanosheets are water-absorbent,

[0043] In some embodiments, the oxidizing solution comprises a hydrogen peroxide solution.

[0044] In some more specific embodiments, the mass fraction of the hydrogen peroxide solution is 15% to 30%. It is understood that the mass fraction of the hydrogen peroxide solution can be, for example, 15%, 17%, 20%, 22%, 25%, 27% or 30%.

[0045] In some embodiments, the base oil includes a polyalphaolefin.

[0046] In some more specific embodiments, the polyalphaolefin includes one or more of PAO2, PAO4, PAO6, and PAO10.

[0047] In some embodiments, the diameter of the black phosphorus nanosheets in the lubricating oil is 50nm to 100nm. It should be noted that before the black phosphorus nanosheets are oxidized, their thickness is nanometers and their diameter can be several hundred nanometers. During the oxidation treatment process of step S1 and step S2, the black phosphorus nanosheets are oxidized and disintegrated, and the diameter of the black phosphorus nanosheets in the lubricating oil finally obtained is 50nm to 100nm, for example, 50nm, 60nm, 70nm, 80nm, 90nm or 100nm.

[0048] In some embodiments, the mass ratio of black phosphorus nanosheets to solvent is 1:(50-200). It is understood that the mass ratio of black phosphorus nanosheets to solvent can be, for example, 1:50, 1:75, 1:100, 1:125, 1:150, 1:175 or 1:200, etc. Specifically, the solvent can include anhydrous ethanol. The present application is beneficial to achieving macroscopic super-lubricating performance of the prepared lubricating oil by controlling the mass ratio of black phosphorus nanosheets to solvent.

[0049] In some embodiments, the volume ratio of the mixture formed by the dispersion of black phosphorus nanosheets in the solvent to the oxidizing solution is (20-100):1. It is understandable that the volume ratio of the mixture formed by the dispersion of black phosphorus nanosheets in the solvent to the oxidizing solution can be, for example, 20:1, 30:1, 40:1, 50:1, 60:1, 70:1, 80:1, 90:1 or 100:1, etc. Specifically, the solvent may include anhydrous ethanol, and the oxidizing solution may include a hydrogen peroxide solution, preferably a hydrogen peroxide solution with a mass fraction of 30%. The present application is beneficial to achieving macroscopic super-lubricating performance of the prepared lubricating oil by controlling the volume ratio of the mixture formed by the dispersion of black phosphorus nanosheets in the solvent to the oxidizing solution.

[0050] In some embodiments, the volume ratio of the dispersion, fatty acid and base oil is 1: (1-10): (1-50). It is understandable that the volume ratio of the dispersion, fatty acid and base oil may include but is not limited to 1: 1: 1, 1: 1: 5, 1: 3: 10, 1: 5: 20, 1: 7: 30, 1: 9: 40 or 1: 10: 50, etc. Specifically, the fatty acid may include one or more of oleic acid, stearic acid, ricinoleic acid and elaidic acid, and the base oil may include polyalphaolefin. The present application is beneficial to achieving macroscopic super-lubricity of the prepared lubricating oil by controlling the volume ratio of the dispersion, fatty acid and base oil.

[0051] In some embodiments, the process of mixing black phosphorus nanosheets, solvent and oxidizing solution in step S1 includes: mixing black phosphorus nanosheets with solvent, performing a first stirring, then mixing with oxidizing solution, and performing a second stirring. The above-mentioned first stirring is conducive to dispersing black phosphorus nanosheets in the solvent, and the second stirring is conducive to fully mixing the solvent dispersed with black phosphorus nanosheets with the oxidizing solution. Specifically, the time of the first stirring is 30min to 50min, for example: 30min, 35min, 40min, 45min or 50min, etc.; specifically, the time of the second stirring is 10min to 60min, for example: 10min, 20min, 30min, 40min, 50min or 60min, etc. More specifically, both the first stirring and the second stirring are magnetic stirring.

[0052] In some embodiments, the process conditions of step S2 include: the mixing time is 15min to 30min, the temperature of the vacuum environment is 80℃ to 100℃, the vacuum degree is -0.06MPa to -0.08MPa, and the drying time is 20min to 60min. It is understandable that the mixing time can be, for example, 15min, 20min, 25min or 30min, the temperature of the vacuum environment can be, for example, 80℃, 85℃, 90℃, 95℃ or 100℃, the vacuum degree can be, for example, -0.06MPa, -0.065MPa, -0.07MPa, -0.075MPa or -0.08MPa, and the drying time can be, for example, 20min, 30min, 40min, 50min or 60min.

[0053] In some embodiments, step S3 includes: magnetically stirring the mixed solution obtained in step S2 for 30 to 60 minutes, and taking an upper oil sample after centrifugal treatment to obtain lubricating oil. It is understood that the magnetic stirring can be 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes or 60 minutes, etc.

[0054] Another embodiment of the present application provides a lubricating oil, which is prepared by the above-mentioned preparation method. It should be noted that the above-mentioned lubricating oil contains black phosphorus oxide, in which the fatty acid is used as an organic carbon source, and the fatty acid is decomposed and carbonized at the interface of the black phosphorus oxide during the friction process, and finally a super-slip interface formed by phosphorus oxide and amorphous carbon is constructed, which reduces the friction coefficient and achieves super-slip at a macroscopic scale.

[0055] Another embodiment of the present application provides a lubricating oil prepared by the above preparation method or the use of the above lubricating oil in preparing a lubricating product. It should be noted that the above lubricating product may include but is not limited to various types of vehicle lubricating oils or lubricating oils suitable for other mechanical equipment to protect mechanical components with friction surfaces from wear. Mechanical components may include but are not limited to pistons, gears, bearings, bearing components or bearing application systems, etc.

[0056] The present application is further described in detail below in conjunction with specific examples and comparative examples. Experimental parameters not specified in the following specific examples are preferably referred to the instructions given in the present application documents, and may also refer to the experimental manual of the art or other experimental methods known in the art, or refer to the experimental conditions recommended by the manufacturer. It is understandable that the instruments and raw materials used in the following examples are more specific, and in other specific embodiments, they may not be limited thereto; the weight of the relevant components mentioned in the embodiments of the present application specification may not only refer to the specific content of each component, but may also represent the proportional relationship of the weight between the components, therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment of the present application specification, it is within the scope disclosed in the embodiment of the present application specification. Specifically, the volume described in the embodiment of the present application specification may be mass units known in the chemical and chemical fields such as μg, mg, g, and kg.

[0057] Example 1

[0058] In this embodiment, the solvent is anhydrous ethanol, the oxidizing solution is 30% by mass of hydrogen peroxide, the fatty acid is oleic acid, and the base oil is polyalphaolefin PAO4.

[0059] The method for preparing the lubricating oil provided in this embodiment comprises the following steps:

[0060] S1. 20 mg of black phosphorus nanosheet powder was dispersed in 2 g of anhydrous ethanol, and magnetically stirred for 30 min. Then, 75 μL of a 30% mass fraction hydrogen peroxide solution was added, and magnetically stirred for 30 min to allow the black phosphorus nanosheets to undergo the first active oxidation to obtain a dispersion;

[0061] S2. Add 5 mL of oleic acid and 5 mL of base oil PAO4 to the above dispersion, stir magnetically for 20 min, and then place in a vacuum drying oven for vacuum drying at 90 ° C to allow the black phosphorus nanosheets to undergo secondary active oxidation while removing anhydrous ethanol. The vacuum drying time is 50 min and the vacuum degree is -0.07 MPa;

[0062] S3. The mixed solution obtained in step S2 is magnetically stirred for 30 minutes, and then centrifuged at 3000 rpm on a centrifuge. After ultrasonic separation, it is allowed to stand for 10 minutes, and an upper oil sample is taken to obtain a lubricating oil containing oxidized black phosphorus nanosheets.

[0063] Example 2

[0064] In this embodiment, the solvent is anhydrous ethanol, the oxidizing solution is 30% by mass of hydrogen peroxide, the fatty acid is oleic acid, and the base oil is polyalphaolefin PAO4.

[0065] The method for preparing the lubricating oil provided in this embodiment comprises the following steps:

[0066] S1. 20 mg of black phosphorus nanosheet powder was dispersed in 2 g of anhydrous ethanol, and magnetically stirred for 30 min. Then, 50 μL of a 30% mass fraction hydrogen peroxide solution was added, and magnetically stirred for 30 min to allow the black phosphorus nanosheets to undergo the first active oxidation to obtain a dispersion;

[0067] S2. Add 5 mL of oleic acid and 5 mL of base oil PAO4 to the above dispersion, stir magnetically for 20 min, and then place in a vacuum drying oven for vacuum drying at 90 ° C to allow the black phosphorus nanosheets to undergo secondary active oxidation while removing anhydrous ethanol. The vacuum drying time is 50 min and the vacuum degree is -0.07 MPa;

[0068] S3. The mixed solution obtained in step S2 is magnetically stirred for 30 minutes, and then centrifuged at 3000 rpm on a centrifuge. After ultrasonic separation, it is allowed to stand for 10 minutes, and an upper oil sample is taken to obtain a lubricating oil containing oxidized black phosphorus nanosheets.

[0069] Example 3

[0070] In this embodiment, the solvent is anhydrous ethanol, the oxidizing solution is 30% by mass of hydrogen peroxide, the fatty acid is oleic acid, and the base oil is polyalphaolefin PAO4.

[0071] The method for preparing the lubricating oil provided in this embodiment comprises the following steps:

[0072] S1. 20 mg of black phosphorus nanosheet powder was dispersed in 2 g of anhydrous ethanol, and magnetically stirred for 30 min. Then, 75 μL of a 30% mass fraction hydrogen peroxide solution was added, and magnetically stirred for 30 min to allow the black phosphorus nanosheets to undergo the first active oxidation to obtain a dispersion;

[0073] S2. Add 12 mL of oleic acid and 30 mL of base oil PAO4 to the above dispersion, stir magnetically for 20 min, and then place in a vacuum drying oven for vacuum drying at 90 ° C to allow the black phosphorus nanosheets to undergo secondary active oxidation while removing anhydrous ethanol. The vacuum drying time is 50 min and the vacuum degree is -0.07 MPa;

[0074] S3. The mixed solution obtained in step S2 is magnetically stirred for 30 minutes, and then centrifuged at 3000 rpm on a centrifuge. After ultrasonic separation, it is allowed to stand for 10 minutes, and an upper oil sample is taken to obtain a lubricating oil containing oxidized black phosphorus nanosheets.

[0075] Example 4

[0076] In this embodiment, the solvent is anhydrous ethanol, the oxidizing solution is 30% by mass of hydrogen peroxide, the fatty acid is oleic acid, and the base oil is polyalphaolefin PAO4.

[0077] The method for preparing the lubricating oil provided in this embodiment comprises the following steps:

[0078] S1. 20 mg of black phosphorus nanosheet powder was dispersed in 2 g of anhydrous ethanol, and magnetically stirred for 30 min. Then, 75 μL of a 30% mass fraction hydrogen peroxide solution was added, and magnetically stirred for 30 min to allow the black phosphorus nanosheets to undergo the first active oxidation to obtain a dispersion;

[0079] S2. Add 24 mL of oleic acid and 130 mL of base oil PAO4 to the above dispersion, stir magnetically for 20 min, and then place in a vacuum drying oven for vacuum drying at 90 ° C to allow the black phosphorus nanosheets to undergo secondary active oxidation while removing anhydrous ethanol. The vacuum drying time is 50 min and the vacuum degree is -0.07 MPa;

[0080] S3. The mixed solution obtained in step S2 is magnetically stirred for 30 minutes, and then centrifuged at 3000 rpm on a centrifuge. After ultrasonic separation, it is allowed to stand for 10 minutes, and an upper oil sample is taken to obtain a lubricating oil containing oxidized black phosphorus nanosheets.

[0081] Example 5

[0082] In this embodiment, the solvent is anhydrous ethanol, the oxidizing solution is 30% by mass of hydrogen peroxide, the fatty acid is oleic acid, and the base oil is polyalphaolefin PAO4.

[0083] The method for preparing the lubricating oil provided in this embodiment comprises the following steps:

[0084] S1. 20 mg of black phosphorus nanosheet powder was dispersed in 4 g of anhydrous ethanol, and magnetically stirred for 30 min. Then, 55 μL of a 30% mass fraction hydrogen peroxide solution was added, and magnetically stirred for 30 min to allow the black phosphorus nanosheets to undergo the first active oxidation to obtain a dispersion;

[0085] S2. Add 30 mL of oleic acid and 30 mL of base oil PAO4 to the above dispersion, stir magnetically for 20 min, and then place in a vacuum drying oven for vacuum drying at 90 ° C to allow the black phosphorus nanosheets to undergo secondary active oxidation while removing anhydrous ethanol. The vacuum drying time is 50 min and the vacuum degree is -0.07 MPa;

[0086] S3. The mixed solution obtained in step S2 is magnetically stirred for 30 minutes, and then centrifuged at 3000 rpm on a centrifuge. After ultrasonic separation, it is allowed to stand for 10 minutes, and an upper oil sample is taken to obtain a lubricating oil containing oxidized black phosphorus nanosheets.

[0087] Example 6

[0088] In this embodiment, the solvent is anhydrous ethanol, the oxidizing solution is 30% by mass of hydrogen peroxide, the fatty acid is oleic acid, and the base oil is polyalphaolefin PAO4.

[0089] The method for preparing the lubricating oil provided in this embodiment comprises the following steps:

[0090] S1. 20 mg of black phosphorus nanosheet powder was dispersed in 1 g of anhydrous ethanol, and magnetically stirred for 30 min. Then, 60 μL of 30% mass fraction hydrogen peroxide solution was added, and magnetically stirred for 30 min to allow the black phosphorus nanosheets to undergo the first active oxidation to obtain a dispersion;

[0091] S2. Add 10 mL of oleic acid and 15 mL of base oil PAO4 to the above dispersion, stir magnetically for 20 min, and then place in a vacuum drying oven for vacuum drying at 90 ° C to allow the black phosphorus nanosheets to undergo secondary active oxidation while removing anhydrous ethanol. The vacuum drying time is 50 min and the vacuum degree is -0.07 MPa;

[0092] S3. The mixed solution obtained in step S2 is magnetically stirred for 30 minutes, and then centrifuged at 3000 rpm on a centrifuge. After ultrasonic separation, it is allowed to stand for 10 minutes, and an upper oil sample is taken to obtain a lubricating oil containing oxidized black phosphorus nanosheets.

[0093] Comparative Example 1

[0094] The preparation method of the lubricating oil provided in this comparative example comprises the following steps:

[0095] 20 mg of black phosphorus nanosheet powder was dispersed into 10 mL of base oil PAO4 and magnetically stirred for 30 minutes to obtain a lubricating oil without oxidized black phosphorus nanosheets.

[0096] Comparative Example 2

[0097] The method is basically the same as Example 1, except that: in step S1, 30% by mass of hydrogen peroxide is not added, and in step S3, lubricating oil free of oxidized black phosphorus nanosheets is obtained.

[0098] Comparative Example 3

[0099] The process is basically the same as Example 1, except that 5 mL of oleic acid in step S2 is replaced by 5 mL of base oil PAO4.

[0100] Friction performance test

[0101] The tribological properties of the lubricating oils prepared in each embodiment and each comparative example were tested using a UMT friction tester. The friction coefficient of the lubricating oil was tested under a load of 1N using a steel ball-steel disk as a friction pair.

[0102] like Figures 1-2As shown, with the steel ball-steel disk as the friction pair, under 1N conditions, the friction coefficient of the super-slip interface constructed based on black phosphorus oxide in Example 1 can be as low as 0.0077 in the atmospheric environment, and the friction coefficient of the super-slip interface constructed based on black phosphorus oxide in Example 2 can be as low as 0.0091 in the atmospheric environment, which fully realizes the super-slip performance at the macro scale. In addition, the super-slip interfaces constructed based on black phosphorus oxide in Examples 3 to 6 have a friction coefficient lower than 0.01 in the atmospheric environment, which also fully realizes the super-slip performance at the macro scale.

[0103] like Figure 3 As shown, with steel ball-steel disk as the friction pair, under 1N condition, the friction coefficient of comparative example 1 is 0.046, and macroscopic super-lubricity is not achieved. In addition, the friction coefficients of comparative examples 2 to 3 are higher than 0.015, and macroscopic super-lubricity is also not achieved.

[0104] In summary, it can be explained that in the preparation method of the lubricating oil of the present application, black phosphorus nanosheets are dispersed by a solvent, and the black phosphorus nanosheets are oxidized by an oxidizing solution. At the same time, the lubricating oil prepared by using fatty acids and base oils significantly reduces the friction coefficient and achieves super-lubricity at a macroscopic scale.

[0105] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0106] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims, and the specification and drawings may be used to interpret the contents of the claims.

Claims

1. A method for preparing lubricating oil, characterized in that: The steps include: S1. Mixing black phosphorus nanosheets, a solvent and an oxidizing solution to perform a primary oxidation treatment on the black phosphorus nanosheets to obtain a dispersion; the mass ratio of the black phosphorus nanosheets to the solvent is 1:(50-200), the volume ratio of the mixture formed by the black phosphorus nanosheets dispersed in the solvent to the oxidizing solution is (20-100):1, the solvent includes anhydrous ethanol, and the oxidizing solution includes a hydrogen peroxide solution; S2. After mixing the dispersion, fatty acid and base oil, drying under vacuum environment to perform secondary oxidation treatment on the black phosphorus nanosheets and remove the solvent; the volume ratio of the dispersion, the fatty acid and the base oil is 1: (1-10): (1-50), the fatty acid includes one or more of oleic acid, stearic acid, ricinoleic acid and elaidic acid, and the base oil includes polyalphaolefin; S3. Separating lubricating oil from the mixed liquid obtained in step S2, wherein the lubricating oil contains black phosphorus oxide.

2. The preparation method according to claim 1, characterized in that: The method comprises at least one of the following features (1) to (2): (1) The mass fraction of the hydrogen peroxide solution is 15% to 30%; (2) The polyalphaolefin includes one or more of PAO2, PAO4, PAO6 and PAO10.

3. The preparation method according to claim 1, characterized in that: The process of mixing the black phosphorus nanosheets, the solvent and the oxidizing solution in step S1 includes: mixing the black phosphorus nanosheets with the solvent, performing a first stirring, and then mixing with the oxidizing solution, and performing a second stirring.

4. The preparation method according to claim 3, characterized in that: The first stirring time is 30 min to 50 min.

5. The preparation method according to claim 3, characterized in that: The second stirring time is 10 min to 60 min.

6. The preparation method according to claim 3, characterized in that: The first stirring and the second stirring are both performed by magnetic stirring.

7. The preparation method according to claim 1, characterized in that: The process conditions of step S2 include: the mixing and stirring time is 15 min to 30 min, the temperature of the vacuum environment is 80° C. to 100° C., the vacuum degree is -0.06 MPa to -0.08 MPa, and the drying time is 20 min to 60 min.

8. The preparation method according to any one of claims 1 to 7, characterized in that Step S3 comprises: magnetically stirring the mixed solution obtained in step S2 for 30 minutes to 60 minutes, taking an upper oil sample after centrifugal treatment, and obtaining the lubricating oil.

9. A lubricating oil, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the lubricating oil prepared by the preparation method according to any one of claims 1 to 8 or the lubricating oil according to claim 9 in the preparation of lubricating products.

Citation Information

Patent Citations

  • Method using polydimethyl siloxane to fast transfer black-phosphorus film

    CN105948005A

  • Method for preparing black phosphorus nanosheets

    CN109019540A

  • Black phosphorene water-based lubricating liquid for titanium alloy rolling and preparation method thereof

    CN112574804A

  • Preparation method of lipophilic black phosphorus lubricating oil

    CN113773892A

  • Magneto-rheological damping fluid composite

    KR100936013B1