Oxidation-resistant hot-formed steel and production method thereof

By optimizing the chemical composition and production process of oxidation-resistant thermoformed steel, the problem of insufficient scale shedding and hardening performance of thermoformed steel is solved, and the high-strength and low-cost thermoforming effect is achieved, which is suitable for complex forming conditions.

CN116200655BActive Publication Date: 2024-11-22PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211589297.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-11-22
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

The surface of hot-formed steel produces loose oxide scales, which easily peels into the mold, reducing the service life of the mold, and the hardening performance of traditional cold-rolled hot-formed steel plates is insufficient.

Method used

Develop an antioxidant thermoformed steel with chemical compositions including C, Mn, Ti, P, S, Si, Cr, B and rare earth elements to control the microstructure and oxidation of the steel through specific hot rolling processes and production processes. The layer ensures the improvement of yield strength, tensile strength and elongation, while reducing the fall of the oxide scale.

Benefits of technology

It realizes high strength and low scale peeling of thermoformed steel, reduces production costs, is suitable for complex forming conditions, and is promoted to other steel types with high surface quality requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116200655B_ABST
    Figure CN116200655B_ABST
Patent Text Reader

Abstract

The present invention discloses an anti-oxidation hot-formed steel and a production method thereof. The microstructure of the steel after hot forming is martensite, the yield strength is ≥1000MPa, the tensile strength is ≥1500MPa, the elongation is ≥6%, and no oxide scale falls off after hot forming, the oxide layer thickness is within 2um, the spot welding process window is ≥1.0KA, and the paint film adhesion level after coating is lower than level 1 required by ISO2409‑2013 standard. The steel provided has a high strength level and can be processed into complex formed parts. Compared with the existing hot-rolled carriage steel, it has the characteristics of high strength and light weight, low production cost, and is suitable for complex forming conditions; compared with conventional 22MnB5 hot-formed steel or coated steel, the parts after hot forming do not need shot blasting or coating treatment, which can avoid micro cracks on the surface of the steel plate caused by improper shot blasting, and has the advantage of low process cost; the hot-rolled oxide scale control method provided can be extended to other steels with high surface quality requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-formed steel, and in particular relates to an anti-oxidation hot-formed steel and a production method thereof. Background Art

[0002] The application of hot-rolled hot-formed steel plates in commercial vehicles has great market potential, but the hot-forming process will produce loose oxide scale on the surface of the steel, which is easy to peel off into the mold, reducing the service life of the mold. Therefore, conventional hot-formed steel is generally shot blasted after mold quenching, or supplied in the state of coated plates, but this increases production costs. Therefore, the development of high-temperature oxidation-resistant hot-formed steel has broad application prospects. Since Si and Cr elements are beneficial to improving the high-temperature oxidation resistance of hot-formed steel, but they will bring serious problems of hot-rolled iron oxide scale. Therefore, it is of great practical significance to design a suitable hot rolling process to reduce hot-rolled iron oxide scale.

[0003] After searching, CN114130842A discloses a method for removing oxide scale from high Cr-Si alloyed 1000-1800MPa grade hot-formed steel, wherein the composition of the steel is: 0.15-0.35% C, 0.8-3.2% Mn, 0.8-2.8% Si, 1.5-3.9% Cr, 0.01-0.05Nb, 0.01-0.05% V, 0.01-0.03% Ti, 0.05-0.15% Cu, and the rest is Fe and unavoidable impurities. A scale removal process combining hydrochloric acid pickling and EPS is provided, wherein pickling is carried out in three stages using hydrochloric acid with a concentration of 60g / L-200g / L and a temperature of 60-95°C. The oxide scale thickness of the steel finally obtained after hot forming is not more than 2um.

[0004] CN114540712A discloses a non-coated reinforced high temperature oxidation resistant hot stamping steel with Ce added, the steel composition is: 0.2-0.4% C, 1.3-2.0% Si, 1.0-1.8% Mn, 0.15-1.5% Cr, 0.01-0.15% Ti, 0.0008-0.004% B, 0.0002-0.01% Ce, Al≤0.05%, S≤0.01%, P≤0.01%, the rest is Fe and inevitable impurities. The steel preparation process includes steelmaking, continuous casting, hot rolling, pickling, cold rolling, annealing, and the steel obtained has a yield strength of ≥1000MPa, a tensile strength of ≥1450MPa, a total elongation of ≥7.0%, and a strength-ductility product of ≥12.0GPa·%.

[0005] In summary, the existing patents do not involve methods for controlling oxidation-resistant hot-formed steel and hot-rolled oxide scale. Summary of the invention

[0006] In order to overcome the defects of the prior art, the present invention develops the production of oxidation-resistant hot-formed steel to address the problem that loose oxide scale will be generated on the surface of steel during the hot forming process, and the oxide scale is easily peeled off into the mold, reducing the service life of the mold; and when hot-formed steel is used for car body plates, the hardenability of traditional cold-rolled hot-formed steel plates is insufficient.

[0007] To achieve the above-mentioned purpose, the present invention provides an oxidation-resistant hot-formed steel, whose chemical composition includes, by weight percentage, C: 0.20-0.24%, Mn: 0.8-2.0%, Ti: 0.015-0.040%, P≤0.015%, S≤0.005%, N≤0.0050%, Si+Cr: 2.0-4.0%, B: 0.0015-0.0040%, rare earth content 0.0015-0.0040%, the rare earth is but not limited to one or more of Ce, Y, La and other elements, and the rest are Fe and unavoidable impurity elements.

[0008] The microstructure of this steel after hot forming is martensite, the yield strength is ≥1000MPa, the tensile strength is ≥1500MPa, the elongation is ≥6%, and there is no oxide scale shedding after hot forming, the oxide layer thickness is within 2μm, the spot welding process window is ≥1.0KA, and the paint film adhesion level after painting is lower than the level 1 required by ISO 2409-2013 standard. The following is an explanation of the main reasons for the limitation of alloy elements in the steel:

[0009] C is an important strengthening element in steel, which has a significant effect on the martensite content and tensile strength of the hot-formed steel plate. When the C content increases, the CCT curve can shift to the right, delaying the transformation of pearlite and bainite to obtain a single martensite structure. Therefore, based on the requirements of structure control and tensile strength, the C content is controlled to 0.20-0.24%.

[0010] Mn plays a role in solid solution strengthening and improving toughness in steel. At the same time, a higher Mn content can improve the hardenability of austenite and reduce the critical cooling rate. However, when the Mn content is too high, it is easy to cause segregation of the ingot and affect the uniformity of the structure. Therefore, the Mn content is controlled to 0.8-2.0%.

[0011] Si is an important interstitial solid solution strengthening element in steel. It can increase the activity of C during the phase transformation process, promote the diffusion of C from ferrite to residual austenite, improve the stability of austenite, and promote the subsequent martensite transformation. At the same time, Si can improve the tempering stability of martensitic steel and reduce the over-aging effect of martensitic steel. In addition, Si can form a dense oxide film during the hot forming process, inhibiting the continued growth of the oxide film on the surface of the steel plate, thereby improving the high-temperature oxidation resistance of the steel.

[0012] Cr can improve the hardenability of steel and promote martensitic transformation. Cr can also improve the high temperature oxidation resistance of steel. Therefore, the present invention requires the addition of Si and Cr, and the Si+Cr content is controlled to be 2.0-4.0%.

[0013] A trace amount of B can significantly improve the hardenability of hot forming steel and obtain a martensitic structure, but when the B content is too high, the risk of grain boundary segregation is greater. Therefore, the B content is controlled to 0.0015-0.0040%.

[0014] Trace rare earth can refine the cast structure by forming fine precipitates, or play a pinning role on the original austenite, promote austenite recrystallization and ferrite refinement. In addition, rare earth is conducive to improving the formation of a dense oxide film during the hot forming process of steel, and improving the bonding strength between the oxide film and the matrix. However, when the rare earth content is high, the risk of forming large-sized oxide or sulfide inclusions is greater. Therefore, the rare earth content is designed to be 0.0015-0.0040%, where rare earth is but not limited to one or more of Ce, Y, La and other elements.

[0015] A small amount of Ti can fix N in steel and form TiN to avoid the formation of BN, thereby increasing the effective content of B. However, the Ti content and N content should not be too high, otherwise the size of the liquid TiN formed will be large, which will easily affect the plasticity of the steel. Therefore, the Ti content is controlled to 0.015-0.040%, and the N content is controlled to 0.0050%.

[0016] A method for producing the oxidation-resistant hot-formed steel adopts a production process of converter smelting-LF refining-RH refining-continuous casting-hot rolling.

[0017] The steel is added with rare earth in the RH vacuum refining process, and the steel liquid O≤0.0015%, S≤0.008% is ensured before adding, and argon blowing treatment is performed after adding rare earth. This is because rare earth is easy to combine with oxygen and sulfur to form large-sized oxide or sulfide inclusions. If rare earth is added in the steelmaking process, it is necessary to ensure that elements such as O and S are controlled at a low level, and it must be after the vacuum process. The problem is solved by adding rare earth in the RH vacuum refining process.

[0018] Furthermore, the thickness of the steel ingot is 200-250 mm.

[0019] Furthermore, the steel is loaded into the slab heating furnace by hot transport and hot charging. Since the steel contains a large amount of hardenability elements such as Si, Cr, and B, the risk of cracking of the cast billet is relatively high when it is cooled at room temperature. Therefore, it is required that the steel billet obtained after continuous casting is loaded into the slab heating furnace by hot transport and hot charging.

[0020] Furthermore, the reheating temperature of the steel slab is 1220-1280°C. In order to loosen the surface oxide scale when the slab is heated, which is beneficial for the subsequent descaling of the slab, thereby reducing the hot rolling oxide scale, a higher slab heating temperature is used. At the same time, a higher heating temperature is conducive to reducing the load of the rolling mill during subsequent rolling, and preventing the rolling mill from crushing the hot rolling oxide scale and pressing it into the surface of the steel plate. Therefore, the slab reheating temperature is controlled to be 1220-1280°C.

[0021] Furthermore, the steel is quickly descaled after being sent out from the heating furnace, and the temperature of the steel billet before descaling is ≥1205°C, and the descaling water pressure is ≥20MPa. Steels with high Si and Cr content are prone to form FeSiO4 (ferroitite phase) during the slab heating process. Its melting point is relatively low, about 1178-1205°C. After solidification from the liquid phase, it is easy to adhere to the iron oxide scale and the steel matrix, and it is difficult to remove in the subsequent descaling process. Therefore, it is necessary to ensure that the FeSiO4 (ferroitite phase) in the slab is completely liquid to facilitate subsequent descaling and removal. It is necessary to control the furnace temperature above 1205°C and increase the descaling water pressure to above 20MPa.

[0022] Furthermore, the steel plate is fully descaled during the rough rolling process, and the overlap between the descaling water sprays is ensured to be between 5-35 mm, so as to ensure that the descaling water fully covers the surface of the steel billet. In order to further remove the possible residual iron oxide scale and / or FeSiO4 (fayalite phase), the steel plate is required to be fully descaled during the rough rolling process, and the overlap between the descaling water sprays is ensured to be between 5-35 mm, so as to ensure that the descaling water fully covers the surface of the steel billet.

[0023] Furthermore, the intermediate billet thickness of the steel plate after rough rolling is 35 to 50 mm.

[0024] Furthermore, the start rolling temperature of the steel plate is 1020-1100°C, the finishing speed is ≥8m / s, and the finishing temperature is 850-890°C. After rolling, laminar cooling is performed, the laminar cooling rate is 15-35°C / s, and the final cooling temperature is 590-630°C. In the finishing rolling process, a lower start rolling temperature (1020-1100°C), a higher final rolling temperature (850-890°C), and a faster rolling speed (≥8m / s) are used to minimize the time the steel plate is in contact with the air before coiling and inhibit the growth of iron oxide scale. However, the finishing rolling temperature cannot be too low, otherwise, the FeO formed by high-temperature rolling will be crushed by rolling, which increases the specific surface area in contact with the air, and further increases the Fe2O3 that is difficult to remove from the oxide layer.

[0025] Furthermore, the steel plate is turned on during the finishing rolling process with medium pressure water, roll anti-stripping water, roll cooling water, and inter-stand cooling water, and the rolls are lubricated, wherein the oil-water volume fraction ratio is 0.7-1.0; the working mileage of the finishing rolls is between 10km and 20km; the cooling water quality used in the laminar cooling process requires Cl - Content ≤100mg / L.

[0026] The state of the rollers during finishing rolling and the surface state of the steel plate also have a great influence on the formation of hot rolling scale. Therefore, the process requirements are: ① The working mileage of the finishing rolling rollers is relatively short, between 10km-20km, so as to avoid serious wear on the roller surface, or the scale on the roller surface falling off to the steel plate, thereby causing the scale on the steel plate surface to increase; ② The rollers are lubricated for rolling, and the ratio is 0.7-1.0, which is also to protect the surface state of the rollers and prevent the scale from falling off or pressing in due to roller vibration. The control of the oil-water volume fraction ratio is to improve the lubrication effect of the roller surface. ③ During the finishing rolling process, the medium-pressure water is turned on to remove the scale on the surface of the steel plate, the anti-stripping water and cooling water of the rollers are turned on to improve the surface state of the rollers, prevent the roller temperature from being too high, and the scale from peeling off after being formed. The cooling water between the racks is turned on to increase the rolling speed and reduce the contact time between the steel plate and the air in the high temperature area.

[0027] There is no descaling measure in the laminar cooling process, so it is impossible to remove the iron oxide scale by descaling like the rolling process. The only way is to reduce the growth of the iron oxide scale as much as possible through process design. First, increase the cooling rate to promote rapid cooling of the steel plate and reduce the time it is in contact with the air in the high temperature section. Secondly, the final cooling temperature should not be too low, because the eutectic reaction temperature of iron oxide (FeO+Fe2O3=Fe3O4) is around 570°C. If the final cooling temperature is lower than 570°C, it will react to form dense Fe3O4, which is not conducive to subsequent pickling. The more ideal state is that the iron oxide scale is controlled to FeO, which is convenient for pickling, so the coiling temperature is required to be controlled at a higher level, that is, 590-630°C. In addition, the water quality of laminar cooling water, especially Cl - The content of Cl promotes the growth of iron oxide scale on steel plates and the formation of iron oxide after corrosion. Therefore, it is required to control Cl - The content is less than 100mg / L.

[0028] The rolling process will not only affect the state of the iron oxide scale on the surface of the steel plate, but also affect the structure and performance of the steel plate. In order to ensure that alloying elements such as Si, Cr, B, and rare earth are fully dissolved, the heating temperature of the slab is designed to be at a higher level, that is, 1220-1280℃. In order to promote the incomplete recrystallization rolling of steel during the finishing rolling process, the finishing rolling temperature is controlled at a lower level, that is, 1020-1100℃, to promote the flattening of the original austenite, accumulate more energy and nucleation points for subsequent phase transformation, and thus promote the refinement of the ferrite structure of the finished product. In order to promote the formation of fine and uniform ferrite structure during the phase transformation process, a higher laminar cooling rate, that is, 15-35℃ / s, is adopted. Since hardenability elements such as Si, Cr, and B are added to the steel, the final cooling temperature should not be too low, otherwise it is easy to form bainite or martensite structure, which increases the difficulty of plate shape control and subsequent pickling and unwinding. Therefore, the final cooling temperature is controlled at 590-630℃.

[0029] Furthermore, the steel plate is coiled into a steel coil after laminar cooling, and then sent to a pickling unit for pickling, the pickling tensile elongation is 1.0-1.4%, and the pickling medium is hydrochloric acid; the thickness of the finished steel obtained after pickling is 2-6mm.

[0030] Furthermore, the process of hot forming of the steel is as follows: holding temperature is 900-950°C, holding time is 5-15min, then mold quenching is performed, and forming is performed while quenching, wherein the mold is provided with a cooling device.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] ① The steel provided by the present invention has a high strength level and can be processed into complex formed parts. Compared with the existing hot-rolled carriage steel, it has the characteristics of adopting high strength and light weight to reduce production costs and is suitable for complex forming conditions.

[0033] ② Compared with conventional 22MnB5 hot-formed steel or coated steel, the steel provided by the present invention does not require shot blasting or coating treatment for hot-formed parts, can also avoid micro cracks on the steel plate surface caused by improper shot blasting process, and has the advantage of low process cost.

[0034] ③ The hot rolling scale control method provided by the present invention can be extended to other steel types with high surface quality requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a diagram showing the oxide layer structure of the test steel after hot forming corresponding to Example 1;

[0036] Figure 2 This is the paint film adhesion rating diagram for the test steel corresponding to Example 1;

[0037] Figure 3 This is the spot welding process window diagram of the test steel corresponding to Example 1. DETAILED DESCRIPTION

[0038] The present invention is further described below in conjunction with specific examples, but the present invention is not limited in any way. To avoid redundant description, the raw materials in the following examples are all commercially available unless otherwise specified, and the methods used are all conventional methods unless otherwise specified.

[0039] Table 1 shows the ingredients of the embodiments of the present invention and the comparative examples, Table 2 shows the production process parameters of the embodiments of the present invention and the comparative examples, and Table 3 shows the mechanical properties and anti-oxidation performance indicators of the steels of the embodiments of the present invention and the comparative examples.

[0040] Table 1 Composition of Examples and Comparative Examples

[0041] C Si Mn P S Cr Ti B Rare Earth N Example 1 0.25 1.93 1.15 0.009 0.002 1.05 0.027 0.0032 0.0022 0.0035 Example 2 0.25 1.47 1.12 0.008 0.003 1.75 0.028 0.0033 0.0025 0.0034 Example 3 0.22 1.68 1.32 0.006 0.004 1.56 0.032 0.0028 0.0030 0.0041 Comparative Example 1 0.25 1.08 0.80 0.010 0.003 0.78 0.010 0.0031 0.0025 0.0058 Comparative Example 2 0.25 1.48 0.80 0.017 0.003 0.81 0.038 0.0031 / 0.0028 Comparative Example 3 0.24 1.42 0.77 0.006 0.002 1.44 0.036 0.0022 / 0.0040

[0042] Table 2 Production process parameters of the embodiments and comparative examples

[0043]

[0044] The hot-formed steels described in Examples 1 to 3 are subjected to hot rolling, laminar cooling, coiling, pickling, quenching, and the descaling system, roll state, laminar cooling water quality and other parameters are strictly controlled during the hot rolling process. The finished steel plates obtained have a yield strength greater than 1000MPa, a tensile strength greater than 1500MPa, an elongation greater than 6%, an oxide layer thickness less than 2μm, a paint film adhesion level lower than level 1, and a spot welding process window greater than 1.0KA.

[0045] Table 2 Production process parameters of embodiments and comparative examples (continued)

[0046]

[0047] Table 3 Mechanical properties and anti-oxidation performance indicators of the examples and comparative examples

[0048]

[0049] Comparative Example 1 has low silicon and chromium contents in the chemical composition and insufficient hardenability, so the yield strength and tensile strength after hot forming are low. At the same time, the heating temperature of the slab is lower than the melting point of the ferrosilicon olivine phase FeSiO4, 1178°C, causing the ferrosilicon olivine to adhere to the matrix and the iron oxide scale formed during heating, resulting in the inability to completely remove the iron oxide scale when the slab is descaled. In addition, the roller anti-scaling water and cooling water are not turned on during the finishing rolling process, and the roller lubrication rolling is not turned on, which will cause the secondary iron oxide scale formed during the hot rolling process to be unable to be completely removed, and ultimately the thickness of the iron oxide scale of the hot-formed finished steel exceeds 2um, and thus the adhesion of the paint film to the steel after painting is reduced.

[0050] No rare earth is added to the chemical composition of Comparative Examples 2 and 3, but rare earth is beneficial to promote the formation of a dense surface oxide layer after hot forming, inhibit the further growth of the oxide layer, and reduce the thickness of the oxide layer. At the same time, the phosphorus removal water pressure of Comparative Example 2 is low, and the iron oxide scale on the surface of the slab cannot be completely removed. Cl in the laminar cooling water of Comparative Example 3 - The content is too high, and the pickling is done by drawing and straightening to promote the shedding of the oxide scale. The improper setting of these process parameters ultimately leads to the oxide scale thickness of the finished steel hot-formed exceeding 2um, and the adhesion of the paint film to the steel is reduced after painting.

[0051] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the disclosed technical content can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.

Claims

1. An oxidation-resistant hot-formed steel, characterized in that: The chemical composition of the oxidation-resistant hot-formed steel includes, by weight percentage, C: 0.20%-0.24%, Mn: 0.8%-2.0%, Ti: 0.015%-0.040%, P≤0.015%, S≤0.005%, N≤0.0050%, Si+Cr: 2.0%-4.0%, B: 0.0015%-0.0040%, rare earth content 0.0015%-0.0040%, the rare earth is but not limited to one or more of Ce, Y, La elements, and the rest is Fe and unavoidable impurity elements; The oxidation layer thickness of the oxidation-resistant hot-formed steel is within 2 μm, and the spot welding process window is ≥1.0 kA; The production method of the oxidation-resistant hot-formed steel adopts a production process of converter smelting-LF refining-RH refining-continuous casting-hot rolling; wherein, The steel billets obtained after continuous casting are sent to the slab heating furnace by hot delivery and hot charging; the slab reheating temperature is 1220℃-1280℃; The billet is quickly descaled after being sent out from the heating furnace. The billet temperature before descaling is ≥1205℃ and the descaling water pressure is ≥20MPa. During the rough rolling process, the scale is removed in the whole pass, and the overlap between the descaling sprays is between 5-35mm; During the finishing rolling process, medium pressure water, roll anti-stripping water, roll cooling water, and inter-stand cooling water are turned on, and the rolls are lubricated, with the oil-water volume fraction ratio of 0.7-1.0; the working mileage of the finishing rolls is between 10-20km; the cooling water quality requirements for the laminar cooling process are Cl - Content ≤100mg / L.

2. The oxidation resistant hot formed steel according to claim 1, characterized in that: Rare earth is added in the RH refining process, and before the addition, O in the molten steel is ≤ 0.0015%, S ≤ 0.008%. After the rare earth is added, argon blowing treatment is performed.

3. The oxidation resistant hot formed steel according to claim 1, characterized in that: The thickness of the intermediate billet after rough rolling of the steel plate is 35-50mm; the starting temperature of the finishing rolling of the steel plate is 1020℃-1100℃, the finishing speed is ≥8m / s, and the finishing temperature is 850℃-890℃; after rolling, laminar cooling is performed, the laminar cooling rate is 15-35℃ / s, and the final cooling temperature is 590℃-630℃.

4. The oxidation resistant hot formed steel according to claim 1, characterized in that: After laminar cooling, the steel plate is coiled into a steel coil and then sent to the pickling unit for pickling. The pickling tensile elongation is 1.0%-1.4%, and the pickling medium is hydrochloric acid. The thickness of the finished steel obtained after pickling is 2-6mm.

5. The oxidation resistant hot formed steel according to claim 1, characterized in that: The hot forming process is: holding temperature 900℃-950℃, holding time 5-15min, then quenching the mold, and forming while quenching, wherein the mold is equipped with a cooling device.