A kind of activated carbon with high nitrogen doping and preparation method thereof

By using ZIF-8 precursor and one-step carbonization activation method, combined with ammonia activator, the problem of controlling heteroatom content and nitrogen doping in activated carbon was solved, and activated carbon with high specific surface area and high nitrogen content was prepared, with excellent Thermal stability and high yield.

CN116216715BActive Publication Date: 2024-11-26CENT SOUTH UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310392062.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-11-26
Estimated Expiration
2043-04-12

AI Technical Summary

Technical Problem

The prior art is difficult to retain the heteroatom content in activated carbon while maintaining a high specific surface area, and it is difficult to control the doping amount of nitrogen elements, affecting the performance and yield of the material.

Method used

ZIF-8, a zeolite imidazole ester skeleton material, was prepared in a methanol-ammonia mixed solution by adjusting the molar ratio of organic imidazole ligand and zinc salt, to control the particle size of ZIF-8, thereby achieving high nitrogen content and ability. The preparation of controlled nano-to-micrometer activated carbon materials is carried out by a one-step carbonization activation method and ammonia gas is used as the activator.

Benefits of technology

The preparation of high-nitrogen doped activated carbon is achieved, with high specific surface area and excellent thermal stability, particle size uniformity, and simple and easy to operate, which improves the performance and yield of activated carbon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116216715B_ABST
    Figure CN116216715B_ABST
Patent Text Reader

Abstract

The invention discloses a kind of activated carbon with high nitrogen doping and its preparation method. The method is to react an organic imidazole ligand and a zinc salt in a mixed solution of methanol-ammonia to obtain a zeolite imidazole ester framework material (ZIF-8), and the zeolite imidazole ester framework material is successively activated by carbonization, cleaned and dried, and obtained. The method realizes the regulation of the nitrogen doping amount in the activated carbon material by accurately controlling the particle size of the prepared ZIF-8, and the nitrogen content is 21.1-26.9at.% after carbonization activation. The method has a simple preparation process, and the obtained activated carbon material has excellent performance, high nitrogen content, large specific surface area, and retains the regular morphology structure of ZIF-8, which has great practical application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an activated carbon material, in particular to an activated carbon material with high nitrogen doping, and also to a preparation method thereof, belonging to the field of environmental protection and new energy material preparation. Background Art

[0002] As a common porous material, activated carbon has a developed pore structure, rich surface elements and stable physical and chemical properties, and is widely used in various fields of production and life. The performance of activated carbon is mainly determined by the specific surface area and surface chemical distribution. The specific surface area provides the main adsorption sites or the internal space for the reaction. The doped chemical elements can significantly improve the properties of the activated carbon surface and enhance the surface affinity. For example, studies have shown that the introduction of nitrogen-containing functional groups such as pyridine and pyrrole can change the charge distribution on the surface of activated carbon, increase the surface polarity, and enhance the interaction strength with the guest molecules through Lewis acid-base interaction, electrostatic interaction or hydrogen bonding.

[0003] The specific surface area can be increased by physical or chemical activation methods. The main principle is to etch the carbon skeleton to form a porous structure by reacting with an activator. Chinese patent CN104310396 solidifies melamine, formaldehyde and F127 or P123 to obtain a nitrogen-containing prepolymer. After high-temperature carbonization, potassium hydroxide is used as an activator. Potassium hydroxide will first be converted into potassium carbonate, and then react with carbon to generate potassium oxide, and finally react to generate metallic potassium element. In the above-mentioned activation process, a large number of heteroatoms such as oxygen and nitrogen in the carbon precursor will also be consumed in large quantities, resulting in a significant decrease in the heteroatom content in the prepared activated carbon, which limits its performance to a certain extent. The doping of activated carbon surface elements is generally achieved by using a heteroatom-rich precursor or by adding a substance containing specific heteroatoms during the activation process. In order to retain heteroatoms to a greater extent, the activation temperature is generally lower than 700°C, so its specific surface area is generally low.

[0004] Therefore, it is of great practical value to provide a method for preparing activated carbon that can maintain a large specific surface area while containing rich heteroatoms. Zeolitic Imidazolate Framework-8 (ZIF-8) is a new type of organic porous material with rich nitrogen atom content. Its raw materials are easily available and the synthesis method is simple. However, it is difficult to control the nitrogen content when using ZIF-8 to prepare activated carbon. Some studies have reported that activated carbon with different nitrogen contents can be obtained by carbonization at different temperatures, but high nitrogen doping can only be achieved at lower temperatures, at which time the specific surface area and pore structure are small; on the other hand, there are also studies that increase the nitrogen content by adding high-nitrogen substances such as urea, melamine, etc. during the carbonization process. However, the addition of these substances will participate in the activation process, resulting in the loss of carbon atoms and a rapid decrease in the yield of activated carbon. Summary of the invention

[0005] In view of the defects of the prior art, the first object of the present invention is to provide an activated carbon material with high nitrogen doping. The material uses ZIF-8 as a precursor, provides abundant nitrogen atoms and a high specific surface area, can still maintain a good morphology and skeleton structure after carbonization, and exhibits excellent thermal stability. By precisely controlling the particle size of the precursor, a high nitrogen content and controllable nano to micron activated carbon material can be obtained.

[0006] The second object of the present invention is to provide a method for preparing activated carbon with high nitrogen doping. The preparation method has a simple process and can achieve control of the particle size of the ZIF-8 precursor from nanometer to micrometer level by adjusting the molar ratio of the raw materials, thereby achieving control of the nitrogen content doped in the activated carbon.

[0007] In order to achieve the above technical objectives, the present invention provides a method for preparing activated carbon with high nitrogen doping, the method comprising reacting an organic imidazole ligand and a zinc salt in a mixed solution of methanol-ammonia water to obtain a zeolite imidazole ester framework material, the zeolite imidazole ester framework material being successively subjected to carbonization activation, washing and drying, and the molar ratio of the organic imidazole ligand and the zinc salt being controlled in the range of 2:1 to 20:1.

[0008] The various properties of ZIF-8 precursor are jointly affected by the type, ratio and solvent properties of the added raw materials. Methanol is often used as a solvent in the ZIF-8 precursor preparation process, so that the prepared ZIF-8 particle size is relatively small, nanometer level, and it is difficult to achieve a large-scale adjustment of particle size. The present invention, on the basis of the mixed solution system of methanol-ammonia, can achieve the particle size control of ZIF-8 precursor from nanometer to micrometer level by changing the raw material ratio. Different reaction ratios can cause the difference in particle size, and excessive neutral 2-methylimidazole can be adsorbed on the surface of the crystal nucleus to slow down the growth of the crystal nucleus, so the particle size of ZIF-8 decreases with the increase of feed ratio. Secondly, the methanol-ammonia mixed solvent is used as a solvent in the present invention. On the one hand, ammonia can be used as a catalyst to induce dimethylimidazole and zinc ions to crystallize rapidly, and methanol can regulate the balance between ZIF-8 nucleation and growth, realizing the rapid and controllable preparation of ZIF-8 crystals. The key to the technology of the present invention is to control the molar ratio of the organic imidazole ligand and the zinc salt. When the molar ratio of the organic imidazole ligand and the zinc salt is high, the particle size of the prepared ZIF-8 precursor is small; when the molar ratio of the organic imidazole ligand and the zinc salt is low, the particle size of the prepared ZIF-8 precursor is large. It is further preferred that when the molar ratio of the organic imidazole ligand and the zinc salt is 8:1, the particle size of the prepared ZIF-8 is 500nm; when the molar ratio of the organic imidazole ligand and the zinc salt is 3.6:1, the particle size of the prepared ZIF-8 is 1μm; when the molar ratio of the organic imidazole ligand and the zinc salt is 2:1, the particle size of the prepared ZIF-8 is 4μm. If the micron-level ZIF-8 is to be controlled, the molar ratio of the organic imidazole ligand and the zinc salt is 2 to 3.6:1. If the particle size of ZIF-8 is to be controlled to be smaller, the molar ratio of the organic imidazole ligand to the zinc salt is preferably 10 to 20:1, more preferably 15 to 20:1.

[0009] As a preferred solution, the organic imidazole ligand is at least one of 2-methylimidazole, 2-ethylimidazole and 2-propylimidazole, and more preferably 2-methylimidazole.

[0010] As a preferred solution, the zinc salt includes zinc acetate and zinc nitrate. Zinc nitrate can be used as an introducing agent for zinc ions, but zinc nitrate is an explosive and hazardous chemical and has certain risks. The present invention further prefers zinc acetate, which has low cost and mild chemical form.

[0011] As a preferred solution, the volume ratio of methanol to ammonia in the methanol-ammonia mixed solution is 6:1 to 10:1, and the mass percentage concentration of ammonia is 5 to 25%. In the present invention, ammonia can induce rapid crystallization of MOF precursors, while methanol can effectively stabilize these precursors and regulate the balance between MOF nucleation and growth. By adjusting the ratio and concentration of methanol and ammonia, rapid and controllable preparation of ZIF-8 crystals can be achieved. Ammonia acts as a catalyst in the reaction. If the concentration of ammonia is too low or the amount is small, the reaction takes a long time to complete. If the concentration is too high or the amount is too high, it is easy to cause an incomplete structure.

[0012] As a preferred solution, the reaction conditions are: reacting at room temperature for 1 to 2 hours under ultrasound assistance. Ultrasonic conditions are conducive to the rapid and complete reaction of the organic imidazole ligand and zinc acetate.

[0013] As a preferred solution, the carbonization activation conditions are: first fill with nitrogen, heat up to 800-1000°C at a heating rate of 1-10°C / min for carbonization, then fill with ammonia, and keep warm for 1-3h. If ZIF-8 is carbonized only in a nitrogen atmosphere, the specific surface area of ​​the obtained activated carbon is low (about 1000m 2 / g), and the nitrogen content is also lower than 20at%. The present invention adopts a one-step carbonization activation method, and only needs to switch the gas when the temperature reaches the setting. The implementation process is simple and easy to operate. Ammonia is used as an activating agent, which can not only improve the pore-forming efficiency, but also introduce additional nitrogen atoms, thereby greatly improving the performance of activated carbon.

[0014] As a preferred solution, the nitrogen gas flow rate is 60-100 mL / min, and the ammonia gas flow rate is 80-150 mL / min. Ammonia is a nitrogen-containing activation gas, and its flow rate affects both the nitrogen content and the pore structure. If the flow rate is too small, the activation effect will not be achieved, or the effect will be uneven; and if the flow rate is too large, the reaction will be too intense, the nitrogen content will increase, but the yield will decrease.

[0015] As a preferred solution, the cleaning process is to first wash with hydrochloric acid having a mass percentage concentration of 5 to 20%, and then repeatedly wash with water.

[0016] As a preferred solution, the drying conditions are: temperature of 60 to 150° C., and drying time of 12 to 36 hours.

[0017] The present invention also provides an activated carbon material with high nitrogen doping, which is obtained by the preparation method.

[0018] As a preferred solution, the particle size of the highly nitrogen-doped activated carbon is 0.5 μm to 4 μm, and the specific surface area is 1903 to 2231 m 2 / g, and the nitrogen content is 21.1~26.9at%.

[0019] Compared with the prior art, the technical solution of the present invention brings the following beneficial technical effects:

[0020] 1. The technical solution of the present invention uses zeolite imidazolate framework material ZIF-8 as a precursor and adopts a new preparation strategy. By precisely controlling the particle size of the ZIF-8 precursor, the nitrogen content doped in the activated carbon can be controlled.

[0021] 2. The technical solution of the present invention can obtain a ZIF-8 precursor with uniform particle size, and adjust the particle size of the ZIF-8 precursor from nanometer to micrometer level, which is beneficial to the subsequent regulation of the nitrogen content of activated carbon. At the same time, a mixed solution of methanol and ammonia water is used as a solvent. On the one hand, ammonia water can act as a catalyst to induce rapid crystallization of dimethylimidazole and zinc ions. On the other hand, methanol can act as a stabilizer to regulate the balance between ZIF-8 nucleation and growth, thereby realizing the rapid and controllable preparation of ZIF-8 crystals, shortening the experimental time, and improving the synthesis efficiency.

[0022] 3. The technical solution of the present invention uses a one-step carbonization activation method, which only requires switching the gas when the temperature reaches the set temperature. The implementation process is simple and easy to operate. Using ammonia as an activator can not only improve the pore-forming efficiency, but also introduce additional nitrogen atoms, greatly improving the performance of activated carbon.

[0023] 4. The highly nitrogen-doped activated carbon prepared by the technical solution of the present invention also has a high specific surface area (1903-2231m 2 / g), with a particle size of 0.5μm to 4μm and a nitrogen content of 21.1 to 26.9at%. At the same time, it retains the regular and ordered skeleton morphology of ZIF-8 and has a certain medium and macropore structure, which is conducive to mass transfer. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The following are scanning electron microscope photos of the ZIF-8 precursor with a particle size of 4 μm and the HNC-3 in Example 3.

[0025] Figure 2 This is the XPS N1s spectrum of HNC-3 in Example 3 of the present invention. DETAILED DESCRIPTION

[0026] The following examples are intended to further illustrate the present invention, rather than to limit the scope of protection of the claims of the present invention.

[0027] Example 1

[0028] 1) Dissolve 6.489g of 2-methylimidazole in 200mL of methanol-ammonia solution and 2.19g of zinc acetate dihydrate in 200mL of methanol-ammonia solution (the volume ratio of methanol to ammonia is 9:1). After they are completely dissolved, mix them evenly and treat them with ultrasound at room temperature for 1-2h. After the reaction is complete, the zeolite imidazole ester framework material is obtained, and the white suspension is collected by centrifugation; then the mixture is repeatedly washed three times with a mixed solution of deionized water and ethanol to obtain the original ZIF-8 precursor with a particle size of 500nm.

[0029] 2) A ZIF-8 precursor with a particle size of 500 nm was placed in a tubular furnace for carbonization activation. The temperature was raised to 900°C at a rate of 5°C / min under a nitrogen gas atmosphere (nitrogen flow rate of 60 mL / min), and then the atmosphere was changed to ammonia (flow rate of 80 mL / min), and the activation was kept warm for 2 hours. After natural cooling, it was taken out to obtain a carbonized product.

[0030] 3) The carbonized product was placed in a sufficient amount of 5% dilute hydrochloric acid, and magnetic stirring was continued for 12 hours to remove residual zinc, and then vacuum filtered. During the process, excess deionized water was used to wash three times until the filtrate was neutral. After vacuum drying at 80° C. for 24 hours, activated carbon with high nitrogen doping was obtained, which was recorded as HNC-1.

[0031] Example 2

[0032] The only difference from Example 1 is the different molar ratio of 2-methylimidazole and zinc acetate. In Example 2, 2.97 g of 2-methylimidazole was dissolved in 40 mL of methanolic ammonia solution, and 2.19 g of zinc acetate dihydrate was dissolved in 360 mL of methanolic ammonia solution to obtain a ZIF-8 precursor with a particle size of 1 μm. The obtained activated carbon was recorded as HNC-2.

[0033] Example 3

[0034] The only difference from Example 1 is the different molar ratio of 2-methylimidazole and zinc acetate. In Example 3, 1.64 g of 2-methylimidazole was dissolved in 50 mL of methanolic ammonia solution, and 2.19 g of zinc acetate dihydrate was dissolved in 150 mL of methanolic ammonia solution to obtain a ZIF-8 precursor with a particle size of 4 μm. The obtained activated carbon was recorded as HNC-3.

[0035] The nitrogen-doped activated carbon materials prepared in Examples 1 to 3 were subjected to nitrogen isothermal adsorption tests (the reference standards are GB / T 21650.2, GB / T 19587, and GB / T 21650.3). The multi-point BET calculated and the results of XPS tests are shown in Table 1.

[0036] Table 1 XPS element distribution and specific surface area of ​​activated carbon samples

[0037]

[0038] As can be seen from Table 1, the XPS surface nitrogen contents of the prepared examples HNC-1, HNC-2 and HNC-3 of the present invention are 21.1at%, 23.5at% and 26.9at%, respectively, which are higher than most of the reported porous carbon materials. Moreover, as the particle size of the ZIF-8 precursor increases, the nitrogen content of the obtained activated carbon shows an upward trend, indicating that the nitrogen element on the surface of the activated carbon can be regulated by precisely changing the particle size. In addition, the highly nitrogen-doped activated carbon obtained by the present invention has a high specific surface area, which is very beneficial for practical applications. Figure 1 It can be seen that the synthesized ZIF-8 precursor has a good crystal structure. After carbonization and activation, the decomposition of the organic part causes its skeleton and particle size to become smaller, but it still retains this regular morphology skeleton structure, indicating its good thermal stability.

[0039] Comparative Example 1

[0040] The only difference from Example 3 is that methanol solution is used instead of the methanol-ammonia mixed solution. The time required for the reaction of the ZIF-8 precursor is significantly longer, and the prepared particle size distribution is uneven. The measured nitrogen content is 22.7 at%.

[0041] Comparative Example 2

[0042] The only difference from Example 3 is that nitrogen atmosphere is used in the carbonization process, and ammonia is not used for activation. The nitrogen content of the prepared activated carbon is 16.7 at%, and the specific surface area is 1262 m 2 / g, which is significantly lower than that in Example 3.

[0043] Comparative Example 3

[0044] The only difference from Example 3 is that melamine is added during the carbonization process, and a nitrogen atmosphere is used for carbonization without using ammonia for activation. The nitrogen content of the prepared sample is 19.7 at%, and the specific surface area is 1963 m 2 / g, which is lower than that in Example 3, and the activated carbon yield is reduced.

[0045] Comparative Example 4

[0046] The only difference from Example 3 is that the carbonized product is activated with potassium hydroxide activator, and the specific surface area is 2903m 2 / g, the nitrogen content is 16.8at%, but the ZIF-8 precursor structure is destroyed and it is an amorphous structure. The results show that the use of potassium hydroxide activator to activate the activated carbon to a certain extent increases the specific surface area, but the nitrogen atom content decreases rapidly.

[0047] Comparative Example 5

[0048] The only difference from Example 3 is that the ratio of methanol to ammonia water used is 4:1, and it is found that the nucleation time of ZIF-8 crystals is significantly increased.

[0049] Comparative Example 6

[0050] The only difference from Example 3 is that the ratio of methanol to ammonia water used is 12:1. It is found that a milky white color quickly appears after the solutions are mixed, indicating that ZIF-8 crystals are quickly generated, but the surface morphology of the porous carbon prepared using it as a precursor is irregular.

Claims

1. A method for preparing highly nitrogen-doped activated carbon, characterized in that: An organic imidazole ligand and a zinc salt are reacted in a mixed solution of methanol-ammonia water to obtain a zeolite imidazole ester framework material, wherein the zeolite imidazole ester framework material is successively subjected to carbonization activation, washing and drying; the molar ratio of the organic imidazole ligand and the zinc salt is controlled within the range of 2:1 to 20:1; the particle size of the zeolite imidazole ester framework material is regulated by controlling the molar ratio of the organic imidazole ligand and the zinc salt, and when the molar ratio of the organic imidazole ligand and the zinc salt is 2 to 3.6:1, a micron-level zeolite imidazole ester framework material is obtained; when the molar ratio of the organic imidazole ligand and the zinc salt is 10 to 20:1, a nanometer-level zeolite imidazole ester framework material is obtained; The volume ratio of methanol to ammonia water in the methanol-ammonia water mixed solution is 6:1-10:1, and the mass percentage concentration of ammonia water is 5-25%.

2. The method for preparing highly nitrogen-doped activated carbon according to claim 1, characterized in that: The organic imidazole ligand is at least one of 2-methylimidazole, 2-ethylimidazole and 2-propylimidazole; The zinc salts include zinc acetate and zinc nitrate.

3. The method for preparing highly nitrogen-doped activated carbon according to claim 1 or 2, characterized in that: The reaction conditions are: reacting at room temperature for 1-2 hours under ultrasound assistance.

4. The method for preparing highly nitrogen-doped activated carbon according to claim 3, characterized in that: The carbonization activation conditions are as follows: firstly, nitrogen is charged, the temperature is raised to 800-1000°C at a heating rate of 1-10°C / min for carbonization, and then ammonia is charged, and the temperature is kept for activation for 1-3 hours.

5. The method for preparing highly nitrogen-doped activated carbon according to claim 4, characterized in that: The nitrogen gas flow rate is 60-100 mL / min, and the ammonia gas flow rate is 80-150 mL / min.

6. The method for preparing highly nitrogen-doped activated carbon according to claim 1, characterized in that: The cleaning process is to first use hydrochloric acid with a mass percentage concentration of 5-20% for washing, and then use water for repeated washing.

7. The method for preparing highly nitrogen-doped activated carbon according to claim 1, characterized in that: The drying conditions are: temperature of 60-150° C., and drying time of 12-36 hours.

8. The method for preparing highly nitrogen-doped activated carbon according to claim 1, characterized in that: The particle size of the highly nitrogen-doped activated carbon is 0.5 μm to 4 μm, and the specific surface area is 1903 to 2231 m 2 / g, and the nitrogen content is 21.1~26.9at%.

Citation Information

Patent Citations

  • Porous activated carbon supported magnesium oxide composite material and preparation method and application thereof

    CN106902742A

  • Preparation method of elemental cobalt composite nitrogen-doped carbon efficient oxygen reduction / oxygen evolution catalyst

    CN110729486A

  • Metal-air battery air electrode and preparation method thereof

    CN111180749A

  • Three-dimensional hierarchical porous nonmetal carbon-based material as well as preparation method and application thereof

    CN112820886A