A kind of tunnel spraying material based on coal gasification slag and its preparation method and application

By mixing materials such as gravel, crude coal gasification slag, fine coal gasification slag and other materials with additives, the problem of roadway pressure under coal gasification slag during deep coal mining is solved, and high-strength and low-cost coal gasification slag is achieved The tunnel spraying improves resource utilization and simplifies the process.

CN116217199BActive Publication Date: 2024-11-15KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211686214.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-27
Publication Date
2024-11-15
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

The tunnel pressure problem caused by coal gasification slag in deep coal mining process is not effectively used as building materials in the existing technology, and there are problems such as high costs, complex processes, and difficult to regulate impurities, which hinder its large-scale utilization.

Method used

Use spray materials composed of gravel, crude coal gasification slag, fine coal gasification slag, cement, slag powder, additive A and additive B, and then sprayed in the tunnel through mixing and stirring, using sodium silicate and hydroxide in additive A. The sodium reacts with the coal gasification slag to form a silicate gel, which increases the strength of the spray material, and forms titanium oxide colloids through tetrabutyl titanate and acetylacetone to enhance compressive strength and adhesion.

Benefits of technology

The high-strength and low-cost preparation of coal gasification slag tunnel spraying was achieved, and the problem of industrial solid waste accumulation was solved. The 3d strength reached 35.3MPa, the 7d strength reached 42.2MPa, and the 28d strength reached 51.8MPa, which simplified the process and improved resource utilization. Rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116217199B_ABST
    Figure CN116217199B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of building materials, and specifically relates to a tunnel spray material based on coal gasification slag, and a preparation method and application thereof. The tunnel spray material based on coal gasification slag; the spray material is composed of the following raw materials in parts by mass: 110-130 parts of gravel, 47-58 parts of coarse coal gasification slag, 23-32 parts of fine coal gasification slag, 7-9 parts of cement, 7-9 parts of slag powder, 1-2 parts of additive A, and 1-2 parts of additive B. 0.3-0.5 parts, 0.1-0.2 parts of fiber, 12-14 parts of water; the additive A is 0.3-0.5 parts of sodium silicate and 0.4-0.6 parts of sodium hydroxide; the additive B is composed of the following raw materials in parts by mass: 0.5-1.5 parts of tetrabutyl titanate and 2.5-3.5 parts of acetylacetone; and the preparation method and application of the spray material solve the problem of a large number of industrial solid waste accumulation, and the preparation process is simple and easy to control. The 3d strength of the coal gasification slag tunnel spray material can reach 35.3MPa, the 7d strength reaches 42.2MPa, and the 28d strength reaches 51.8Mpa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to a tunnel spray material based on coal gasification slag, and a preparation method and application thereof. Background Art

[0002] With the rapid development of coal chemical industry, the emission of gasification slag is increasing day by day. At present, the large-scale disposal and utilization of gasification slag has attracted widespread attention mainly in the development and utilization of carbon materials, the preparation of ceramic materials, and the preparation of aluminum / silicon-based products. Although the economic benefits are relatively significant, they are all in the laboratory research or expansion test stage. The main problems are high cost, complicated process, difficult to control impurities, small downstream market, etc., and large-scale utilization cannot be achieved.

[0003] Due to the special composition of coal gasification slag, the large-scale use of coal gasification slag needs to consider its possibility as a building material. When entering the deep coal mining stage, the tunneling will be affected by the mining pressure of the overlying rock layer and the surrounding goaf during the construction process, which brings hidden dangers to the safe production of coal mines.

[0004] Therefore, in view of the above-mentioned technical problems and defects, it is urgently necessary to design and develop a tunnel spraying material based on coal gasification slag and its preparation method and application. Summary of the invention

[0005] In order to overcome the above-mentioned deficiencies and difficulties in the prior art, the object of the present invention is to provide a tunnel spraying material based on coal gasification slag and a preparation method and application thereof.

[0006] The first object of the present invention is to provide a tunnel injection material based on coal gasification slag;

[0007] The second object of the present invention is to provide a method for preparing spray material for tunnels based on coal gasification slag;

[0008] The third object of the present invention is to provide an application of spraying materials for tunnels based on coal gasification slag;

[0009] The first object of the present invention is achieved in that the spray material is composed of the following raw materials in parts by mass:

[0010] 110-130 parts of gravel, 47-58 parts of coarse coal gasification slag, 23-32 parts of fine coal gasification slag, 7-9 parts of cement, 7-9 parts of slag powder, 1-2 parts of additive A, 0.3-0.5 parts of additive B, 0.1-0.2 parts of fiber, 12-14 parts of water;

[0011] The additive A is 0.3-0.5 parts of sodium silicate and 0.4-0.6 parts of sodium hydroxide; the additive B is composed of the following raw materials in parts by mass: 0.5-1.5 parts of tetrabutyl titanate and 2.5-3.5 parts of acetylacetone.

[0012] The second object of the present invention is achieved in that the method comprises the following steps:

[0013] (1) mixing gravel, coarse coal gasification slag, fine coal gasification slag, cement, slag powder and fiber uniformly to obtain a solid mixture;

[0014] (2) The solid mixture is mixed with additive A, additive B and water, and stirred, and after curing, a coal gasification slag-based tunnel spray material is obtained.

[0015] The third object of the present invention is achieved in that the spray material is sprayed in the tunnels in the deep coal mining stage.

[0016] The scheme of the present invention uses a tunnel spray material based on coal gasification slag; the spray material is composed of the following raw materials in parts by mass: 110-130 parts of gravel, 47-58 parts of coarse coal gasification slag, 23-32 parts of fine coal gasification slag, 7-9 parts of cement, 7-9 parts of slag powder, 1-2 parts of additive A, 0.3-0.5 parts of additive B, 0.1-0.2 parts of fiber, and 12-14 parts of water; the additive A is 0.3-0.5 parts of sodium silicate and 0.4-0.6 parts of sodium hydroxide; the additive B is composed of the following raw materials in parts by mass: 0.5-1.5 parts of tetrabutyl titanate and 2.5-3.5 parts of acetylacetone; and the preparation method and application of the spray material solve the problem of a large amount of industrial solid waste accumulation, and the preparation process is simple and easy to control;

[0017] In addition, the 3d strength of the coal gasification slag tunnel spraying can reach 35.3MPa, the 7d strength can reach 42.2MPa, and the 28d strength can reach 51.8Mpa. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a schematic cross-sectional view of a coal gasification slag tunnel injection test block obtained in Example 4 of the present invention after curing for 3 days;

[0019] Figure 2 This is a schematic cross-sectional view of a coal gasification slag tunnel injection test block obtained in Example 4 of the present invention after curing for 7 days;

[0020] Figure 3 This is a schematic cross-sectional view of a coal gasification slag tunnel injection test block obtained in Example 4 of the present invention after curing for 28 days;

[0021] Figure 4 The present invention is a schematic flow chart of a method for preparing spraying material for tunnels based on coal gasification slag. DETAILED DESCRIPTION

[0022] The present invention is further described below in conjunction with the accompanying drawings, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.

[0023] As attached Figure 1-4 As shown, the scheme of the present invention provides a tunnel spray material based on coal gasification slag, wherein the spray material is composed of the following raw materials in parts by mass: 110-130 parts of gravel, 47-58 parts of coarse coal gasification slag, 23-32 parts of fine coal gasification slag, 7-9 parts of cement, 7-9 parts of slag powder, 1-2 parts of additive A, 0.3-0.5 parts of additive B, 0.1-0.2 parts of fiber, and 12-14 parts of water;

[0024] The additive A is 0.3-0.5 parts of sodium silicate and 0.4-0.6 parts of sodium hydroxide; the additive B is composed of the following raw materials in parts by mass: 0.5-1.5 parts of tetrabutyl titanate and 2.5-3.5 parts of acetylacetone.

[0025] The particle size of the coarse coal gasification slag is in the range of 0.5 to 5 mm; the specific surface area of ​​the fine coal gasification slag is greater than 300 m 2 / kg.

[0026] The stone is a continuously graded stone with a diameter of 1 to 30 mm, and the compressive strength of the stone is greater than 100 MPa.

[0027] The slag powder is S95 grade slag powder, and the specific surface area of ​​the slag powder is greater than or equal to 450m 2 / kg, the density of the slag powder is 2.7~3.5g / cm 3 .

[0028] The length of the fiber is 3-17 mm; the fiber is made of polypropylene resin.

[0029] In order to achieve the purpose of the scheme of the present invention, the scheme of the present invention also provides a method for preparing a tunnel spray material based on coal gasification slag, and the method comprises the following steps:

[0030] (1) mixing gravel, coarse coal gasification slag, fine coal gasification slag, cement, slag powder and fiber uniformly to obtain a solid mixture;

[0031] (2) The solid mixture is mixed with additive A, additive B and water, and stirred, and after curing, a coal gasification slag-based tunnel spray material is obtained.

[0032] The mixing and stirring speed in step (1) is 25-35 r / min, and the mixing time is 30-50 s; the mixing and stirring speed in step (2) is 25-35 r / min, and the mixing time is 30-50 s.

[0033] The humidity of the curing in step (2) is 95±2%, and the curing temperature is 20±2°C.

[0034] In order to achieve the purpose of the scheme of the present invention, the scheme of the present invention also provides an application of a tunnel spray material based on coal gasification slag, wherein the spray material is sprayed in the tunnel in the deep coal mining stage.

[0035] Specifically, in a specific embodiment of the scheme of the present invention, a coal gasification slag tunnel spraying material is prepared from raw materials comprising the following mass parts: 110-130 parts of gravel, 47-58 parts of coarse coal gasification slag, 23-32 parts of fine coal gasification slag, 7-9 parts of cement, 7-9 parts of slag powder, 1-2 parts of additive A, 0.3-0.5 parts of additive B, 0.1-0.2 parts of fiber, and 12-14 parts of water.

[0036] The stone is selected from 1-30mm continuous graded stone, and the compressive strength of the stone is greater than 100MPa; the particle size range of the coarse coal gasification slag is 0.5-5mm;

[0037] The specific surface area of ​​the fine coal gasification slag is greater than 300m 2 / kg. The cement is 425 cement, and the three-day compressive strength is greater than 30MPa. The slag powder is S95 grade slag powder, and the specific surface area of ​​the slag powder is greater than or equal to 450m 2 / kg, the density of the slag powder is 2.7~3.5g / cm 3 ;

[0038] The additive A is 0.3-0.5 parts of sodium silicate and 0.4-0.6 parts of sodium hydroxide. The additive B is prepared from the following raw materials in parts by weight: 0.5-1.5 parts of tetrabutyl titanate and 2.5-3.5 parts of acetylacetone.

[0039] The type of the fiber is polypropylene resin, and the length of the fiber is 3 to 17 mm.

[0040] The method for preparing coal gasification slag tunnel spraying material provided by the present invention comprises the following steps:

[0041] (1) Mixing gravel, coarse coal gasification slag, fine coal gasification slag, cement, slag powder and fiber uniformly to obtain a solid mixture;

[0042] (2) Mix the solid mixture with additive A, additive B and water, and obtain the coal gasification slag tunnel spray material after curing. The stirring speed of the mixing in step (1) is 25~35r / min, and the mixing time is 30~50s. The stirring speed of the mixing in step (2) is 25~35r / min, and the mixing time is 30~50s. The humidity of the curing in step (2) is 95±2%, and the curing temperature is 20±2℃.

[0043] The principle of the present invention is: the formula of the coal gasification slag solid waste synthetic concrete material of the present invention is obtained through theory and experiment, wherein:

[0044] 1. Slag powder can achieve higher strength through the action of additives, and can also fill the micropores of the spray material, so that the spray material has higher strength. Among them, the comparison between Example 2 and Example 3 can draw the conclusion that the strength is improved.

[0045] 2. Tetrabutyl titanate and acetylacetone in the additive can produce titanium oxide colloid, which greatly improves the compressive strength of the spray material, and at the same time can improve the adhesion of the spray material and reduce the rebound rate of the spray material. This conclusion can be drawn by comparing Example 3 with Example 4.

[0046] 3. The sodium hydroxide and sodium silicate in the additive react with the coal gasification slag to generate silicate gel and hardened silicate needle-shaped crystals, thereby improving the strength of the sprayed material. This conclusion can be drawn by comparing Example 2 with Example 3.

[0047] The present invention provides a coal gasification slag roadway spraying material, which is prepared from the following raw materials by mass: 110-130 parts of gravel, 47-58 parts of coarse coal gasification slag, 23-32 parts of fine coal gasification slag, 7-9 parts of cement, 7-9 parts of slag powder, 1-2 parts of additive A, 0.3-0.5 parts of additive B, 0.1-0.2 parts of fiber, and 12-14 parts of water. The coal gasification slag roadway spraying material prepared by the present invention has low cost, solves the problem of a large amount of industrial solid waste accumulation, and improves resource utilization; the 3d strength of the coal gasification slag roadway spraying material reaches 35.3MPa, the 7d strength reaches 42.2MPa, and the 28d strength reaches 51.8MPa.

[0048] The present invention provides a method for preparing coal gasification slag tunnel spraying material, comprising mixing stone, coal gasification slag, slag powder, cement and fiber in sequence to obtain a solid raw material; mixing a solid raw material activator and water, and curing to obtain the coal gasification slag tunnel spraying material. The present invention has a simple preparation process, high production efficiency, simple and stable operation, convenient control, and easy realization of automated operation.

[0049] In the present invention, the mass fraction of the gravel is 110 to 130 parts, more preferably 115 to 125 parts. The mass fraction of the crude coal gasification slag is 47 to 58 parts, more preferably 50 to 54 parts.

[0050] In the present invention, the mass fraction of the fine coal gasification slag is 23 to 32 parts, more preferably 28 to 30 parts, the mass fraction of the slag powder is 7 to 9 parts, and the mass fraction of the cement is 7 to 9 parts.

[0051] In the present invention, the additive A is 1-2 parts. The additive A is 0.3-0.5 parts of sodium silicate and 0.4-0.6 parts of sodium hydroxide, more preferably 0.4 parts of sodium silicate and 0.6 parts of sodium hydroxide.

[0052] In the present invention, the additive B is 0.3-0.5 parts, the tetrabutyl titanate is 0.5-1.5 parts, and the acetylacetone is 2.5-3.5 parts, and more preferably, the tetrabutyl titanate is 1 part and the acetylacetone is 3 parts.

[0053] The mass fraction of the fiber is 0.1 to 0.2 parts, more preferably 0.12 to 0.18 parts, and more preferably 0.15 parts. The mass fraction of the water is 12 to 14 parts.

[0054] In the present invention, the stone is selected from 1-30mm continuous graded stone, and the compressive strength of the stone is greater than 100MPa; the particle size range of the coarse coal gasification slag is 0.5-5mm; the specific surface area of ​​the fine coal gasification slag is greater than 300m2 / kg. The cement is 425 cement, and the three-day compressive strength is greater than 30MPa.

[0055] The slag powder is S95 grade slag powder, the specific surface area of ​​the slag powder is greater than or equal to 450m2 / kg, and the density of the slag powder is 2.7-3.5g / cm3; the type of the fiber is polypropylene resin, and the length of the fiber is 3-17mm

[0056] The present invention also provides a method for preparing coal gasification slag tunnel spraying material, comprising the following steps:

[0057] (1) Mixing gravel, coal gasification slag, slag powder, cement and fiber in sequence to obtain a solid mixture;

[0058] (2) The solid mixture is mixed with an activator and water, and after curing, the coal gasification slag tunnel spraying material is obtained.

[0059] In step (1), the stirring speed of the mixing is preferably 25-35 r / min, more preferably 28-32 r / min, and more preferably 30 r / min; the mixing time is 30-50 s, and more preferably 40 s. In step (2), the solid raw material is mixed with the activator and water, and the stirring speed is preferably 25-35 r / min, more preferably 28-32 r / min, and more preferably 30 r / min; the mixing time is 30-50 s, and more preferably 40 s.

[0060] The material mixed in step (2) is added into the mold, and a layer of plastic wrap is covered on the surface of the material. After 24 hours, it is taken out of the mold and then cured. The humidity of the curing in step (2) is 95±2%, and the curing temperature is 20±2°C.

[0061] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0062] Embodiment 1~5

[0063] In Examples 1-5, the raw materials are weighed according to the proportions described in Table 1, and the activator is dissolved in water to obtain an activator solution; first, gravel and coarse coal gasification slag are poured into a mixer, and then fine coal gasification slag, slag powder, cement, and fiber are added in sequence and stirred at a stirring speed of 30 r / min for 40 seconds, the mixture is stirred evenly, and then the activator and water are added in sequence to obtain a uniformly mixed fluidized spray material.

[0064] Then pour the mixture into a 100*100*100mm plastic triple mold for molding. After 24 hours, take the concrete block out of the mold and put it into a curing box with a humidity of 95% and a temperature of 20°C for curing. Take it out after 3, 7, and 28 days to test the compressive strength. The compressive strength is measured in accordance with GB / T17671-1999, and the test results are shown in the following table.

[0065]

[0066] It can be seen from the above table that the 28d compressive strength of the filling materials prepared in Examples 5-10 is greater than 44 MPa, which meets the strength requirements of tunnel spraying. Figures 1 to 3 They are cross-sectional pictures of Example 4 at 3d, 7d and 28d of maintenance respectively. Through observation, it is found that the various components of the spraying material are mixed evenly and tightly combined, and have very high compressive strength, which is very beneficial for tunnel construction and coal mining operations.

[0067] Compared with the shotcrete used for tunnels with application number 202110429102.5, the compressive strength of the present invention is 51.8 MPa, which is much greater than its strength of 38.7 MPa. At the same time, the rebound rate of the present invention (8.9~9.7) is also significantly lower than its rebound rate (10.7~11.1). At the same time, the present invention makes full use of industrial waste gasification slag, reduces costs, and realizes the green and environmentally friendly construction concept.

Claims

1. A kind of tunnel spraying material based on coal gasification slag, It is characterized in that The spray material is made of 110-130 parts by weight of gravel, 47-58 parts of coarse coal gasification slag, 23-32 parts of fine coal gasification slag, 7-9 parts of cement, 7-9 parts of slag powder, 1-2 parts of additive A, 0.3-0.5 parts of additive B, 0.1-0.2 parts of fiber, and 12-14 parts of water; the additive A is 0.3-0.5 parts of sodium silicate and 0.4-0.6 parts of sodium hydroxide; the additive B is composed of 0.5-1.5 parts of tetrabutyl titanate and 2.5-3.5 parts of acetylacetone; the particle size range of the coarse coal gasification slag is 0.5-5 mm, and the specific surface area of ​​the fine coal gasification slag is greater than 300 m 2 / kg; the stone is a continuously graded stone of 1-30mm and the compressive strength of the stone is greater than 100MPa; the slag powder is S95 grade slag powder with a specific surface area greater than or equal to 450m 2 / kg, density is 2.7~3.5g / cm 3 ; The fiber is a polypropylene resin with a length of 3 to 17 mm.

2. A method for preparing the spray material for tunnel based on coal gasification slag according to claim 1, It is characterized in that The preparation method comprises the following steps: (1) Mix gravel, coarse coal gasification slag, fine coal gasification slag, cement, slag powder and fiber evenly, and stir at a speed of 25-35 r / min for 30-50 s to obtain a solid mixture; (2) The solid mixture is mixed with additive A, additive B and water, and stirred at a speed of 25 to 35 r / min for 30 to 50 seconds. After curing, the coal gasification slag-based tunnel spray material is obtained.

3. An application of the coal gasification slag-based tunnel spraying material according to claim 1, It is characterized in that The coal gasification slag-based tunnel spraying material is sprayed on the tunnel in the deep coal mining stage.