Through photothermal dual curing and epoxy resin compounding technology, the problems of high volume shrinkage and slow curing speed of UV cross-linked adhesives are solved, low volume shrinkage and fast light curing are achieved, meeting the needs of high-speed communication optical modules precise positioning requirements.

CN116218439BActive Publication Date: 2024-10-29WUHAN HUAGONG GENUINE OPTICS TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310156702.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-23
Publication Date
2024-10-29
Estimated Expiration
2043-02-23

AI Technical Summary

Technical Problem

Existing UV cross-linked adhesives have a large volume shrinkage during the curing process, resulting in micro-displacement, and the curing speed is not enough to meet the rapid positioning requirements of high-speed communication optical modules.

Method used

The low volume shrinkage UV cross-linked rapid positioning adhesive using photothermal dual curing uses epoxy oligomers, reactive diluents, tackifying resins, silicon carbide powder, glass beads, photoinitiators, and thermal initiators. It is combined with a microcapsule foaming agent to control the volume shrinkage during the curing process, and the light curing speed is increased by compounding three-membered ring epoxy resin and four-membered ring epoxy resin.

Benefits of technology

The volume shrinkage is controlled within 1%, the light curing time is shortened to less than 20 seconds, meeting the precise positioning requirements, and supplementary curing by thermal curing ensures full curing of the entire area, improving production efficiency and positioning accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the field of adhesive technology, and in particular to a low volume shrinkage UV cross-linked rapid positioning adhesive, a preparation method and an application thereof; in terms of weight percentage, the adhesive comprises: 20-40% epoxy polymer, 10-35% active diluent, 5-15% tackifying resin, 10-40% silicon carbide powder, 5-30% glass microspheres, 1-5% photoinitiator, 1-5% thermal initiator, 0.1-1% microcapsule foaming agent, and 0.1-1.0% leveling agent. The adhesive of the present application reduces volume shrinkage by introducing a microcapsule foaming agent, and the volume shrinkage of the improved adhesive is controlled within 1%; by adopting a compounding method of a ternary ring epoxy resin monomer and a quaternary ring epoxy resin monomer, the light curing speed is shortened to within 20 seconds. The glue prepared by the present invention can be used in the field of rapid and precise positioning, and is particularly suitable for rapid positioning and bonding during the coupling process of electronic components in the optical communication industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesives, and in particular to a low volume shrinkage UV cross-linking rapid positioning adhesive and a preparation method and application thereof. Background Art

[0002] The coupling and bonding of electronic components in the optical communication industry requires the use of precision positioning adhesives. With the rapid development of the communication industry, the demand for high-speed communication optical modules is becoming more and more urgent, and the requirements for precision positioning type pre-fixed adhesives are becoming higher and higher. On the one hand, the glue is required to be able to be photocured and positioned in the shortest time to meet production efficiency. On the other hand, the glue curing process is required to produce no micro-displacement to meet the needs of precise positioning. Therefore, a low volume shrinkage UV cross-linking fast positioning adhesive is urgently needed to solve the above problems.

[0003] Commonly used acrylic UV cross-linked adhesives have a volume shrinkage rate of about 6-8% due to the curing polycondensation. The volume shrinkage rate is relatively large, resulting in micro displacement during the curing process. The volume shrinkage rate of epoxy UV cross-linked adhesives is about 2% because the ring opening can compensate for the volume shrinkage caused by the polycondensation. The adhesive disclosed in patent CN114989730 A uses expansion monomers as the main raw material and compensates for the curing volume shrinkage through the volume gain of epoxy resin ring opening. The expansion monomers mainly include spirocyclic carbonates, spirocyclic carbonates, bicyclic carbonates, bicyclic lactones, etc. Most expansion monomers are still in the research stage. Only a small number of products such as 3,9-dihydroxymethyl-3',9'-diethyl-1,5,7,11-tetraoxaspiro[5,5]undecane have been industrialized, and the price is high, so they have not yet been widely promoted and applied.

[0004] Currently, the UV cross-linking adhesives commonly used in the industry mostly use three-membered ring epoxy resins. The curing speed of such monomers is limited, and fast positioning curing (i.e., light curing time) still requires 30-60s, while the curing reaction of oxetane-based four-membered epoxy monomers is too fast and cannot be controlled during application. In order to improve production efficiency, it is necessary to further shorten the light curing reaction time of the adhesive while reducing the volume shrinkage rate. Summary of the invention

[0005] In order to solve the above problems, on the one hand, the present invention provides a low volume shrinkage UV cross-linking rapid positioning adhesive, which can be used for precise and rapid positioning. The adhesive adopts a dual light and heat curing method, and no by-products are produced during and after the curing process. It is green and environmentally friendly, and it can be quickly positioned by light curing. In areas where light cannot reach, thermal curing is used for supplementary curing, and the application range is wide. The adhesive uses a foaming agent to offset the volume shrinkage of the cationic polymerization process, and its performance fully meets the needs of rapid curing and precise positioning of electronic components.

[0006] To achieve the above-mentioned purpose, the present invention provides a low volume shrinkage UV cross-linking rapid positioning adhesive, which comprises, by weight percentage, 20-40% epoxy polymer, 10-35% reactive diluent, 5-15% tackifying resin, 10-40% silicon carbide powder, 5-30% glass microbeads, 1-5% photoinitiator, 1-5% thermal initiator, 0.1-1% microcapsule foaming agent, and 0.1-1.0% leveling agent.

[0007] Furthermore, the epoxy-based oligomer includes a ternary ring epoxy resin monomer and a quaternary ring epoxy resin monomer, wherein the mass of the quaternary ring epoxy resin monomer is 10 to 40% of the mass of the ternary ring epoxy resin monomer.

[0008] In the present application, the epoxy polymer in the adhesive is prepared by compounding ternary ring epoxy resin and quaternary ring epoxy resin monomers. The curing speed of the ternary ring epoxy resin monomer is slow and cannot meet the demand for rapid curing, while the quaternary ring epoxy resin monomer is not suitable for use in this type of adhesive due to its too fast curing reaction speed. The present application appropriately increases the photocuring reaction speed by adding a small amount of quaternary ring epoxy resin monomer to the ternary ring epoxy resin monomer to meet the increasing demand for rapid production.

[0009] Furthermore, the three-membered ring epoxy resin monomer is at least one of 3,4-epoxycyclohexylcarboxylic acid-3,4-epoxycyclohexylmethyl ester (UVR6110) and bis(3,4-epoxycyclohexylmethyl) adipate (UVR6128), and the four-membered ring epoxy resin monomer is at least one of 3-ethyl-3-oxetanecarbinol and methacrylate oxetane.

[0010] Furthermore, the active diluent is one or more of triethylene glycol divinyl ether (DEV-3), 1,4-cyclohexyl dimethanol divinyl ether (CHVE), 4-hydroxybutyl vinyl ether (HBVE), dodecyl vinyl ether (DDVE), glycerol carbonate propenyl ether, 1,4-cyclohexyl dimethanol divinyl ether, 1,4-dihydroxymethylcyclohexane divinyl ether, trimethylolethane trivinyl ether, 1-propenyl ether, 1-butenyl ether and 1-pentenyl ether.

[0011] In the present application, the mass percentage of the active diluent in the adhesive is 10 to 35%. On the one hand, the active diluent plays a diluting role, so that the adhesive has a viscosity for construction. On the other hand, the active diluent is reactive. When exposed to light, it copolymerizes with the oligomer to form a network structure, which can increase the photocuring rate of the system. The active diluent in the present application is a vinyl ether compound, which can be one of the above-mentioned compounds, or a mixture of two or more, and is selected according to actual needs.

[0012] In the present application, the mass percentage of the tackifying resin in the adhesive is 5-15%, and the tackifying resin is used to adjust the thixotropic properties of the system to achieve the purpose of suitable application. The tackifying resin can be a core-shell rubber modified epoxy resin toughening agent, MX125, MX153 or MX167 of Japan KANEKA.

[0013] In the present application, silicon carbide powder is used to adjust the hardness of the system, and the silicon carbide powder is 1250 mesh ultrafine silicon carbide powder.

[0014] In the present application, glass microspheres are used to adjust the specific gravity of the system, and the glass microspheres are hollow glass microspheres with a diameter of 10 to 25 μm.

[0015] Further, the photoinitiator is a cationic initiator of sulfonium salt and iodonium salt, specifically one or more of bis(4-dodecylbenzene)iodonium hexafluorophosphate, 4,4-dimethyldiphenyliodonium hexafluorophosphate, (4-octyloxyphenyl)phenyliodonium hexafluoroantimonate, bis(4-tert-butylphenyl)iodonium hexafluorophosphate, 4-isobutylphenyl-4-methylphenyliodonium hexafluoroantimonate, (4-octyloxyphenyl)phenyliodonium hexafluoroantimonate, and (5-toluenesulfonyloxyimide-5H-thiophene-2-ylidene)-(4-methoxyphenyl)-acetonitrile.

[0016] Furthermore, the thermal initiator is one or more of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, diethylaminopropylamine, aliphatic modified amines, aromatic amines, phthalic anhydride, and dicyandiamide.

[0017] Furthermore, the microcapsule foaming agent in the adhesive releases nitrogen after heating, so that the volume of the system increases. The core of the microcapsule foaming agent is one or more of diazoaniline, benzenesulfonic acid hydrazide, p-toluenesulfonic acid hydrazide, 2,4-disulfonylhydrazide toluene, 4,4-oxybisbenzenesulfonylhydrazide, and azodicarbonamide.

[0018] Furthermore, the leveling agent is polysiloxane, specifically one of BYK-377, BYK-378, BYK-3455, and BYK-3760.

[0019] On the other hand, the present invention also provides a method for preparing the UV cross-linking rapid positioning adhesive with low volume shrinkage as described above, comprising the following steps:

[0020] S1: Add active diluent, silicon carbide powder, glass beads and microcapsule foaming agent into a high-speed mixer respectively, and mix and stir for 10-15 minutes until the mixture is uniform;

[0021] In the above mixing process, in order to prevent the solid raw materials from sinking to the bottom and causing uneven mixing, when adding materials, the liquid component is added first, and then the solid component is added, and the materials are added while stirring to make the materials mixed more evenly.

[0022] S2: adding epoxy oligomer and tackifying resin to the mixture of step S1, mixing and stirring for 10-15 minutes until the mixture is uniform;

[0023] S3: Add photoinitiator, thermal initiator and leveling agent to the mixture in step S2, and mix and stir for 10-15 minutes;

[0024] S4: placing the mixture obtained in step S3 in a degassing machine, and evacuating the mixture at a vacuum degree of -0.1 MPa for 15 to 25 minutes to obtain the low volume shrinkage UV cross-linking rapid positioning adhesive.

[0025] On the other hand, the present invention also provides an application of the low volume shrinkage UV cross-linking rapid positioning adhesive as described above, wherein the adhesive is applied, preliminarily cured by light, and then supplementally cured by heating, so that areas that cannot be reached by light can also be fully cured.

[0026] Due to the adoption of the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0027] 1) The low volume shrinkage UV cross-linked rapid positioning adhesive provided by the present invention effectively improves the photocuring reaction speed of the adhesive by compounding the ternary ring epoxy resin monomer and the quaternary ring epoxy resin monomer, and the photocuring speed is shortened to within 20 seconds, meeting the increasing demand for rapid positioning; by controlling the ratio of the ternary ring epoxy resin monomer and the quaternary ring epoxy resin monomer, a suitable reaction speed is obtained, that is, the defect of the slow reaction speed of the ternary ring epoxy resin monomer is overcome, and the problem of the excessively fast reaction speed of the quaternary ring epoxy resin monomer is avoided;

[0028] 2) The low volume shrinkage UV cross-linking rapid positioning adhesive provided by the present invention adopts a microcapsule foaming agent to offset the volume reduction problem in the polymer polycondensation process, so that the volume shrinkage of the adhesive is controlled within 1%, meeting the needs of precise positioning; epoxy resin is used as the main base material, and the volume shrinkage is relatively small compared with acrylic resin. Without adding a microcapsule foaming agent, the volume shrinkage of the epoxy system can be controlled to within 2%. The use of an epoxy resin system can effectively control the amount of microcapsule foaming agent used; the control of the amount of microcapsule foaming agent added can effectively control the loose porous structure caused by the foaming itself, and then the defects of cohesive strength and material density, so that the adhesive with the microcapsule foaming agent can still have a suitable cohesive strength and hardness; and the gas released by the microcapsule foaming agent when heated is nitrogen, which is pollution-free to the environment;

[0029] 3) The low volume shrinkage UV cross-linking rapid positioning adhesive provided by the present invention adopts a non-volatile reactive active diluent, which is environmentally friendly and safe. In addition, the reactive active diluent can further increase the density of the film and has a certain tonic effect on the decrease in cohesive strength caused by adding a microcapsule foaming agent;

[0030] 4) The low volume shrinkage UV cross-linking rapid positioning adhesive provided by the present invention uses silicon carbide powder as a functional filler to supplement the hardness of the system, and can further reduce the reduction in the cohesive strength and hardness of the system caused by the microcapsule foaming agent. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The invention provides a low volume shrinkage UV cross-linking rapid positioning adhesive. The adhesive comprises, by weight percentage, 20-40% of epoxy oligomer, 10-35% of active diluent, 5-15% of tackifying resin, 10-40% of silicon carbide powder, 5-30% of glass microbeads, 1-5% of photoinitiator, 1-5% of thermal initiator, 0.1-1% of microcapsule foaming agent, and 0.1-1.0% of leveling agent; wherein the epoxy oligomer is a compound of a ternary ring epoxy resin monomer and a quaternary ring epoxy resin monomer. The preparation method of the adhesive is described below through a specific implementation method. Embodiment 1

[0033] This embodiment provides a low volume shrinkage UV cross-linking rapid positioning adhesive, and the preparation method thereof comprises the following steps:

[0034] S1: Add 52 g 1,4-cyclohexyl dimethanol divinyl ether (CHVE), 32 g 1250 mesh ultrafine silicon carbide powder, 14 g hollow glass microspheres with a particle size of 15 µm, and 0.6 g benzenesulfonic acid hydrazide into a small high-speed blender, and mix and stir for 15 to 35 min at a stirring rate of 100-1200 RPM / MIN until the mixture is uniformly mixed. Note that cyclohexyl dimethanol divinyl ether should be added first, and then other materials to prevent the powder from sinking to the bottom;

[0035] S2: Add 12 g of oxetane methacrylate, 50 g of 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate (UVR6110), and 25.2 g of MX153 to the mixture in step S1, and continue stirring and dispersing for 10 to 20 minutes until the mixture is uniformly mixed;

[0036] S3: 5.8 g of bis(4-dodecylbenzene)iodonium hexafluorophosphate, 3.8 g of methyl hexahydrophthalic anhydride, and 0.6 g of BYK-377 are added to the mixture in step S2, and the mixture is stirred and dispersed for 10 to 15 minutes until the mixture is uniformly mixed.

[0037] S4: placing the solution obtained in step S3 in a degassing machine, and evacuating the solution for 15 to 25 minutes at a vacuum degree of -0.1 MPa to finally obtain a UV cross-linked rapid positioning adhesive with low volume shrinkage.

[0038] Embodiment 2

[0039] This embodiment provides a low volume shrinkage UV cross-linking rapid positioning adhesive, and the preparation method thereof comprises the following steps:

[0040] S1: Add 48g triethylene glycol divinyl ether (DEV-3), 38g 1250 mesh ultrafine silicon carbide powder, 11g 15µm hollow glass microspheres, and 0.6g azodicarbonamide into a small high-speed blender and mix for 10-15min at a stirring rate of 100-1200 RPM / MIN until the mixture is uniform.

[0041] S2: Add 16 g of 3-ethyl-3-oxetanol, 50 g of bis(3,4-epoxycyclohexylmethyl) adipate (UVR6128), and 18.5 g of MX153 to the mixture in step S1, and continue stirring and dispersing for 10 to 20 minutes until the mixture is uniformly mixed;

[0042] S3: Add 6.3 g of bis(4-tert-butylphenyl)iodonium hexafluorophosphate, 3.8 g of methyl hexahydrophthalic anhydride, and 0.8 g of BYK-3455 to the mixture obtained in step S2, and continue to stir and disperse for 10 to 15 minutes until the mixture is evenly dispersed;

[0043] S4: placing the solution obtained in step S3 in a degassing machine, and evacuating the solution for 15 to 25 minutes at a vacuum degree of -0.1 MPa to finally obtain a UV cross-linked rapid positioning adhesive with low volume shrinkage.

[0044] Embodiment 3

[0045] This embodiment provides a low volume shrinkage UV cross-linking rapid positioning adhesive, and the preparation method thereof comprises the following steps:

[0046] S1: Add 66.2 g 1,4-cyclohexyl dimethanol divinyl ether, 34 g 1250 mesh ultrafine silicon carbide powder, 16 g 15µm hollow glass microspheres, and 0.6 g azodicarbonamide into a small high-speed mixer, and mix and stir at high speed for 15 to 30 min at a stirring rate of 100-1200 RPM / MIN until the mixture is uniformly mixed;

[0047] S2: Add 16 g of oxetane methacrylate, 42 g of 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate (UVR6110), and 14 g of MX125 to the mixture of step S1, and continue stirring for 10 to 20 minutes until the mixture is uniform;

[0048] S3: Add 5.4 g of 4-isobutylphenyl-4-methylphenyliodonium hexafluoroantimonate, 4.8 g of methyl hexahydrophthalic anhydride, and 1.0 g of BYK-377 to the mixture obtained in step S2, and continue stirring and mixing for 10 to 15 minutes until the mixture is uniform;

[0049] S4: placing the solution obtained in step S3 in a degassing machine, and evacuating the solution for 15 to 25 minutes at a vacuum degree of -0.1 MPa to finally obtain a UV cross-linked rapid positioning adhesive with low volume shrinkage.

[0050] Embodiment 4

[0051] This embodiment provides a low volume shrinkage UV cross-linking rapid positioning adhesive, and the preparation method thereof comprises the following steps:

[0052] S1: Add 55.8g triethylene glycol divinyl ether (DEV-3), 37g 1250 mesh ultrafine carbonized fiber powder, 13g 15µm hollow glass microspheres, and 0.8g p-toluenesulfonic acid hydrazide into a small high-speed mixer, and stir and disperse for 15-30min at a stirring rate of 100-1200 RPM / MIN until the mixture is uniformly dispersed;

[0053] S2: Add 17 g of oxetane methacrylate, 48 g of bis(3,4-epoxycyclohexylmethyl) adipate (UVR6128), and 16 g of MX167 to the mixture obtained in step S1, and continue stirring and dispersing for 10 to 20 minutes until the mixture is uniformly dispersed;

[0054] S3: Add 6.4 g (4-octyloxyphenyl)phenyl iodonium hexafluoroantimonate, 4.9 g methyl hexahydrophthalic anhydride, and 1.1 g BYK-3760 to the mixture in step S2, and continue stirring and mixing for 10 to 15 minutes until the mixture is uniformly stirred;

[0055] S4: placing the solution obtained in step S3 in a degassing machine, and evacuating the solution for 15 to 25 minutes at a vacuum degree of -0.1 MPa to finally obtain a UV cross-linked rapid positioning adhesive with low volume shrinkage.

[0056] Comparative Example 1

[0057] The components and preparation method of Comparative Example 1 are different from those of Example 1 in that no benzenesulfonic acid hydrazide and methacrylic acid oxetane ester are added in Comparative Example 1, and the added mass of 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate (UVR6110) is 62 g. The rest is the same as Example 1 and will not be repeated here.

[0058] Comparative Example 2

[0059] The components and preparation method of Comparative Example 2 are different from those of Example 2 in that no azodicarbonamide and 3-ethyl-3-oxetanemethanol are added in Comparative Example 2, and the added amount of bis(3,4-epoxycyclohexylmethyl) adipate (UVR6128) is 60 g.

[0060] Comparative Example 3

[0061] The components and preparation method of Comparative Example 3 are different from those of Example 3 in that azodicarbonamide and methacrylic acid oxetane are not added in Comparative Example 3, and the added amount of 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate (UVR6110) is 58 g.

[0062] Comparative Example 4

[0063] The components and preparation method of Comparative Example 4 are different from those of Example 4 in that p-toluenesulfonic acid hydrazide and methacrylate oxetane are not added in Comparative Example 4, and the added amount of bis(3,4-epoxycyclohexylmethyl adipate) (UVR6128) is 65 g.

[0064] In Comparative Examples 1, 2, 3 and 4, no quaternary ring epoxy resin monomer and microcapsule foaming agent were added, and the amount of ternary ring epoxy resin monomer was adjusted.

[0065] Comparative Example 5

[0066] Comparative Example 5 is a commercially available acrylic ester low volume shrinkage UV cross-linked rapid positioning adhesive from a certain company, with a brand name of BEN 5651-H.

[0067] The performance comparison of the low volume shrinkage UV cross-linking rapid positioning adhesive of the embodiment and the comparative example is as follows:

[0068] Table 1

[0069]

[0070] In Table 1, the volume shrinkage rate was tested using a 0.01mg electronic balance and the drainage method; the light curing conditions were tested using DSC; the hardness was tested using the D-type Shore durometer method; the specific gravity was tested using a specific gravity balance; and the elastic modulus was tested using the DMA tensile mode.

[0071] From the above, we can see that by neutralizing the ternary ring epoxy resin monomer and compounding the quaternary ring epoxy resin monomer, the light curing time can be effectively reduced, thereby achieving rapid positioning; by adding microcapsule foaming agent, the volume shrinkage rate can be effectively reduced, and precise positioning can be achieved; thus, the electronic components can be quickly and accurately positioned on the substrate; for areas that cannot be reached by light, thermal curing can be supplemented to achieve complete curing of the adhesive. The thermal curing time can be set according to actual needs.

[0072] Those skilled in the art will appreciate that the present invention can be implemented in many other specific forms without departing from the spirit and scope of the present invention. Although embodiments of the present invention have been described, it should be understood that the present invention should not be limited to this embodiment, and those skilled in the art can make changes and modifications within the spirit and scope of the present invention as defined by the appended claims.

Claims

1. A low volume shrinkage UV cross-linking rapid positioning adhesive, characterized in that: Measured by weight percentage, the adhesive includes: 20-40% epoxy polymer, 10-35% active diluent, 5-15% tackifying resin, 10-40% silicon carbide powder, 5-30% glass beads, 1-5% photoinitiator, 1-5% thermal initiator, 0.1-1% microcapsule foaming agent, and 0.1-1.0% leveling agent; the epoxy polymer includes a ternary ring epoxy resin monomer and a quaternary ring epoxy resin monomer, wherein the mass of the quaternary ring epoxy resin monomer is 10-40% of the mass of the ternary ring epoxy resin monomer.

2. The low volume shrinkage UV cross-linking rapid positioning adhesive according to claim 1, characterized in that: The three-membered ring epoxy resin monomer is at least one of 3,4-epoxycyclohexylcarboxylic acid-3,4-epoxycyclohexylmethyl ester and bis(3,4-epoxycyclohexylmethyl) adipate, and the four-membered ring epoxy resin monomer is at least one of 3-ethyl-3-oxetanol and methacrylate oxetanyl ester.

3. The low volume shrinkage UV cross-linking rapid positioning adhesive according to claim 1, characterized in that: The active diluent is one or more of triethylene glycol divinyl ether, 1,4-cyclohexyl dimethanol divinyl ether, 4-hydroxybutyl vinyl ether, dodecyl vinyl ether, glycerol carbonate propenyl ether, 1,4-cyclohexyl dimethanol divinyl ether, 1,4-dihydroxymethylcyclohexane divinyl ether, trimethylolethane trivinyl ether, 1-propylene ether, 1-butylene ether and 1-pentene ether.

4. The low volume shrinkage UV cross-linking rapid positioning adhesive according to claim 1, characterized in that: The photoinitiator is a cationic initiator of sulfonium salt and iodonium salt, specifically one or more of bis(4-dodecylbenzene)iodonium hexafluorophosphate, 4,4-dimethyldiphenyliodonium hexafluorophosphate, (4-octyloxyphenyl)phenyliodonium hexafluoroantimonate, bis(4-tert-butylphenyl)iodonium hexafluorophosphate, 4-isobutylphenyl-4-methylphenyliodonium hexafluoroantimonate, (4-octyloxyphenyl)phenyliodonium hexafluoroantimonate, and (5-p-toluenesulfonyloxyimide-5H-thiophene-2-ylidene)-(4-methoxyphenyl)-acetonitrile.

5. The low volume shrinkage UV cross-linking rapid positioning adhesive according to claim 1, characterized in that: The thermal initiator is one or more of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, diethylaminopropylamine, aliphatic modified amines, aromatic amines, phthalic anhydride, and dicyandiamide.

6. The low volume shrinkage UV cross-linking rapid positioning adhesive according to claim 1, characterized in that: The core of the microcapsule foaming agent is one or more of diazoaniline, benzenesulfonic acid hydrazide, p-toluenesulfonic acid hydrazide, 2,4-disulfonylhydrazide toluene, 4,4-oxybisbenzenesulfonylhydrazide and azodicarbonamide.

7. The low volume shrinkage UV cross-linking rapid positioning adhesive according to claim 1, characterized in that: The leveling agent is polysiloxane, specifically one of BYK-377, BYK-378, BYK-3455 and BYK-3760.

8. A method for preparing a UV cross-linked rapid positioning adhesive with low volume shrinkage as claimed in any one of claims 1 to 7, characterized in that: The steps include: S1: Add active diluent, silicon carbide powder, glass beads and microcapsule foaming agent into a high-speed mixer respectively, and mix and stir for 10-15 minutes until the mixture is uniform; S2: adding epoxy oligomer and tackifying resin to the mixture of step S1, mixing and stirring for 10-15 minutes until the mixture is uniform; S3: Add photoinitiator, thermal initiator and leveling agent to the mixture in step S2, and mix and stir for 10-15 minutes; S4: placing the mixture obtained in step S3 in a degassing machine, and evacuating the mixture at a vacuum degree of -0.1 MPa for 15 to 25 min to obtain the low volume shrinkage UV cross-linking rapid positioning adhesive.

9. An application of the low volume shrinkage UV cross-linking rapid positioning adhesive as claimed in any one of claims 1 to 7, characterized in that: The adhesive is applied, initially cured by a UV light source, and then supplemented by heating to achieve complete curing of the adhesive.

Citation Information

Patent Citations

  • Intumescent UV crosslinking low-stress adhesive and preparation method thereof

    CN114989730A

  • Preparation method of carbon-dioxide-base polyurea high polymer material

    CN104650322A

  • Thin plate reinforcing adhesive matrix composition for welding, and preparation method thereof, and reinforcing adhesive sheet

    CN110511705A