A method for preparing calcium-sodium based grease
By using butter, palmitoleic acid and stearic acid as multi-component fat materials, the saponification reaction process is optimized, and the problems of low drop points of calcium-based grease and complex sodium-based grease processes are solved, and the calcium-based grease is improved The high temperature resistance and shear stability achieve high performance and low cost grease preparation.
Patent Information
- Application Number
- CN202211667709.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-23
AI Technical Summary
The existing calcium-based grease has low drop points, which limits its application range. Sodium-based grease has a high usage temperature, but it has complex preparation process, a wide variety of raw materials, a rough appearance and poor high temperature resistance.
Using butter, palmitoleic acid and stearic acid as multi-component fat materials, calcium-sodium-based grease is prepared through saponification reaction, optimize the proportion of thickening agents and process conditions, improve the thickening of grease, high temperature resistance and shearing of grease Make sure to be stable.
The drop point, high temperature resistance and shear stability of calcium-sodium-based grease are significantly improved, and a grease with transparent appearance and good corrosion resistance is obtained, which simplifies the preparation process and reduces costs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lubricating grease, and in particular to a method for preparing calcium-sodium based lubricating grease. Background Art
[0002] Calcium-based grease has a long history, mature production technology, simple production facilities and low cost, so it is very popular. It is well known that calcium-based grease has excellent colloidal stability, but the problem of low dropping point seriously limits its practical application range. At the same time, sodium-based grease has a higher operating temperature. Therefore, attempts were made to select fat materials with different ratios, combine the two greases, and prepare calcium-sodium-based greases that have the performance of both calcium-based greases and sodium-based greases.
[0003] In the prior art related to calcium-based grease, CN109135899A discloses a calcium-sodium-based grease for stamping machinery, which includes a base grease obtained by thickening a base oil with a thickener composed of fatty calcium soap, fatty sodium soap, and an organic compound containing polyurea. CN106479635A discloses a wide-temperature water-resistant and rust-proof rail top grease composition, which includes a 70% to 90% by mass ratio of MVI300 base oil and a 10% to 30% poly-α-olefin compound as a base oil, combined with a variety of composite additives. Although the performance of the above-mentioned grease has been improved to a certain extent, there are still disadvantages such as complex preparation process, a wide variety of raw materials, rough appearance of the grease, or poor performance such as high temperature resistance, and there is room for further improvement. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a calcium-sodium based grease and a preparation method thereof. The present invention introduces tallow as a necessary fat material into the system, which is conducive to the thickening of the grease into fat. However, the grease prepared using tallow as a raw material has a rough appearance and poor high temperature resistance. To this end, the present invention further explores and provides a multi-component fat material for preparing different calcium-sodium based grease experimental schemes.
[0005] In a first aspect, the calcium-sodium based grease provided by the present invention comprises, by weight: 70 to 95 parts of a base oil and 5 to 30 parts of a thickener, wherein the base oil is a mineral oil, the thickener is prepared by saponification of an alkali and a fat material, the alkali comprises sodium hydroxide and calcium hydroxide, and the fat material comprises tallow, palmitic acid and stearic acid in a mass ratio of 1:0:0 to 10:1:3.
[0006] The various calcium-sodium based greases provided by the present invention include a single-component fat material, a two-component fat material and a three-component fat material. The present invention finds that by using tallow as the fatty acid in the thickener in the above manner, it is more conducive to the thickening of the grease into fat. Tallow is selected as the necessary fat material, and palmitic acid is introduced into the system to be combined with tallow to further improve the fineness and high temperature resistance of the grease. Further, when stearic acid is introduced into the system, the high temperature resistance and shear stability of the calcium-sodium based grease of the specific three-component fat material are effectively improved, and the overall performance is better than that of the previous scheme.
[0007] Preferably, the fatty material is tallow, palmitoleic acid and stearic acid.
[0008] In order to further improve the comprehensive performance of calcium-sodium based grease in various aspects, the present invention also optimizes the ratio of the three-component fat materials and provides the following preferred scheme.
[0009] Preferably, the mass ratio of tallow, palmitic acid and stearic acid is 1:1:1 to 8:1:3, most preferably 7:1:2.
[0010] Further preferably, the mass ratio of the sodium hydroxide to the calcium hydroxide is 8-20:1-5, preferably 13:3.
[0011] The thickener of tallow, palmitic acid and stearic acid in a specific ratio and sodium hydroxide in the above mass ratio and the calcium hydroxide saponification can cooperate well with the mineral oil 500SN of the present invention to obtain a calcium-sodium based grease, which significantly improves the dropping point of the grease and has a small change in cone penetration after working 10,000 times, and has better high temperature resistance and shear stability.
[0012] Preferably, the base oil is 500SN; preferably, the kinematic viscosity of the base oil at 40°C is 90-107 mm 2 / s, viscosity index not less than 95, pour point not less than -18°C. The mineral oil 500SN with the preferred parameters in the present invention can better cooperate with the thickener of the three-component fatty material. The 500SN base oil has a high viscosity index and the viscosity is less affected by temperature, which further improves the stability of the grease.
[0013] Further preferably, the calcium-sodium based grease is composed of a base oil and a thickener, with the total mass of the grease composition as the basis, 75-90% of the base oil, 10-25% of the thickener, preferably 85-90% of the base oil, 10-15% of the thickener. Under the preferred usage ratio, the mechanical stability of the grease is better.
[0014] In a second aspect, the present invention also provides a method for preparing the calcium-sodium based grease, comprising: mixing a mixed solution of base oil and fat material with a mixed aqueous solution of sodium hydroxide and calcium hydroxide, performing a saponification reaction, heating, performing a constant temperature treatment, thickening into fat and oil pressing.
[0015] Preferably, the preparation of the mixed aqueous solution of sodium hydroxide and calcium hydroxide comprises mixing sodium hydroxide and calcium hydroxide with water in the same mass ratio; and / or, the preparation of the mixed solution of base oil and fat material comprises mixing base oil and fat material at a temperature of 85-90° C. In the present invention, by adopting the above preparation method, the preparation process can be simplified, and the method of the present invention has low requirements on production facilities, has greater cost advantages, and the prepared grease has excellent comprehensive performance.
[0016] More preferably, the saponification reaction is a two-stage saponification reaction; preferably, the temperature of the first stage is 105-110° C., the reaction time is 50-70 min, and the temperature of the second stage is 110-115° C., the reaction time is 110-130 min.
[0017] In the present invention, by adopting the optimized two-stage saponification reaction, the water evaporation loss is reduced and the saponification reaction is made more complete.
[0018] More preferably, after the saponification reaction is completed, the temperature is raised to 205-215° C. and the temperature is kept constant for 5-10 minutes.
[0019] Further preferably, the thickening and fat-forming process includes mixing the material treated at a constant temperature with the quenching oil, reducing the temperature to 170-175° C., further reducing the temperature to 130° C., adding the rear adjustment oil, and stirring.
[0020] In the present invention, by adopting the optimized constant temperature treatment and thickening and fat-forming treatment, the soap fiber structure of the best calcium-sodium based grease can be obtained, and the stability of the grease is further improved.
[0021] Preferably, the quenching oil is a base oil that accounts for 3 / 8 of the total mass of the base oil, and the post-adjusting oil is a base oil that accounts for 1 / 8 of the total mass of the base oil.
[0022] Further preferably, the preparation method of the calcium-sodium based grease includes: heating part of the base oil and the fat material to 85-90°C in a reactor to form a uniform mixed solution; continuing to heat, mixing with a mixed aqueous solution of sodium hydroxide and calcium hydroxide at 95-100°C, reacting at 105-110°C for 50-60min, and then reacting at 110-115°C for 120-130min; then heating the material to 205-215°C, and treating at a constant temperature for 5-10min; adding quenching oil until the temperature drops to 170-175°C, and then cooling to 125-135°C, adding the rear oil, stirring, and rolling the oil two to three times. The use of the optimized process and conditions of this application is conducive to further improving the comprehensive performance of the grease.
[0023] The beneficial effects of the present invention are at least that: the calcium-sodium based grease provided by the present invention has a transparent appearance, excellent high temperature performance, corrosion resistance and colloidal stability, and has broad market prospects; at the same time, the raw materials used in the present invention are low in cost, and the industrial production facilities and processes of the grease are simple, which has cost advantages. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The technical means used in the examples are conventional means known to those skilled in the art. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased through regular channels.
[0026] In the embodiment of the present invention, the kinematic viscosity of the base oil 500SN used at 40°C is 96 mm 2 / s, viscosity index 99, pour point -18℃. Example 1
[0027] This embodiment provides a calcium-sodium based grease composition, which is prepared by the following method:
[0028] 1. Dissolve 26g of sodium hydroxide and 6g of calcium hydroxide in 32g of water and stir well to form a uniform mixed alkali solution.
[0029] 2.Put 200g of butter and 800g of 500SN base oil into a 5L reactor, heat it to 85~90℃, and keep it at this temperature for 5~10min until the butter is completely dissolved.
[0030] 3. Heat the reactor to 100°C, add the mixed alkali solution, and after the temperature is constant, heat it up in stages (Stage 1: 105~110°C, reaction for 60 minutes. Stage 2: 110~115°C, continue reaction for 120 minutes).
[0031] 4. After saponification is completed, continue to raise the temperature to 210℃ and keep the temperature constant for 5~10 minutes.
[0032] 5. Add 600g 500SN base oil and cool it down to 170~175℃, then continue to cool it down to 130℃, add 200g 500SN base oil and stir evenly. Then, reduce the temperature to 80~90℃, press the oil three times and get the finished product. Example 2
[0033] This embodiment provides a calcium-sodium based grease composition, which is prepared by the following method:
[0034] 1. Dissolve 26g of sodium hydroxide and 6g of calcium hydroxide in 32g of water and stir well to form a uniform mixed alkali solution.
[0035] 2. Put 800g 500SN base oil, 180g tallow and 20g palmitoleic acid into a 5L reactor, heat to 85~90℃, and keep the temperature constant for 5~10min until the tallow is completely dissolved.
[0036] 3. Heat the reactor to 100°C, add the mixed alkali solution, and after the temperature is constant, heat it up in stages (Stage 1: 105~110°C, reaction for 60 minutes. Stage 2: 110~115°C, continue reaction for 120 minutes).
[0037] 4. After saponification is completed, continue to raise the temperature to 210℃ and keep the temperature constant for 5~10 minutes.
[0038] 5. Add 600g500SN base oil and cool it down to 170~175℃, then continue to cool it down to 130℃, add 200g500SN base oil and stir evenly. Then, reduce the temperature to 80~90℃, press the oil three times and get the finished product. Example 3
[0039] This embodiment provides a calcium-sodium based grease composition, which is prepared by the following method:
[0040] 1. Dissolve 26g of sodium hydroxide and 6g of calcium hydroxide in 32g of water and stir well to form a uniform mixed alkali solution.
[0041] 2. Put 800g base oil, 140g tallow, 20g palmitic acid and 40g stearic acid into a 5L reactor, heat to 85~90℃, and keep the temperature constant for 5~10min until the tallow is completely dissolved.
[0042] 3. Heat the reactor to 100°C, add the mixed alkali solution, and after the temperature is constant, heat it up in stages (Stage 1: 105~110°C, reaction for 60 minutes. Stage 2: 110~115°C, continue reaction for 120 minutes).
[0043] 4. After saponification is completed, continue to raise the temperature to 210℃ and keep the temperature constant for 5~10 minutes.
[0044] 5. Add 600g500SN base oil and cool it down to 170~175℃, then continue to cool it down to 130℃, add 200g500SN base oil and stir evenly. Then, reduce the temperature to 80~90℃, press the oil three times and get the finished product. Comparative Example 1
[0045] The difference between this comparative example and Example 1 is that the tallow used in the thickener is replaced by an equal amount of palm oil. Comparative Example 2
[0046] The difference between this comparative example and Example 1 is that the tallow used in the thickener is replaced by an equal amount of stearic acid. Comparative Example 3
[0047] The difference between this comparative example and Example 1 is that the tallow used in the thickener is replaced by an equal amount of castor seed oil. Comparative Example 4
[0048] The difference between this comparative example and Example 1 is that the tallow used in the thickener is replaced by an equal amount of hydrogenated castor oil. Comparative Example 5
[0049] The difference between this comparative example and Example 1 is that the tallow used in the thickener is replaced by an equal amount of 12-hydroxystearic acid. Comparative Example 6
[0050] The difference between this comparative example and Example 2 is that the palmitoleic acid used in the thickener is replaced by an equal amount of stearic acid. Comparative Example 7
[0051] The difference between this comparative example and Example 2 is that the palmitoleic acid used in the thickener is replaced by an equal amount of castor seed oil. Comparative Example 8
[0052] The difference between this comparative example and Example 2 is that the palmitoleic acid used in the thickener is replaced by an equal amount of 12-hydroxystearic acid. Example 4
[0053] The difference between this embodiment and embodiment 3 is that 140 g of tallow, 20 g of palmitoleic acid and 40 g of stearic acid used in the thickener are replaced with 160 g of tallow, 20 g of palmitoleic acid and 20 g of stearic acid. Example 5
[0054] The difference between this embodiment and embodiment 3 is that 140 g of tallow, 20 g of palmitoleic acid and 40 g of stearic acid used in the thickener are replaced with 120 g of tallow, 20 g of palmitoleic acid and 60 g of stearic acid.
[0055] Experimental example
[0056] The dropping point and cone penetration of the single-component fat material were tested. The test plan and main analysis data are shown in Table 1.
[0057]
[0058] It can be seen from the results that oil-soap separation or no fat formation occurs in Comparative Examples 2, 3, 4 and 5; and in Comparative Example 1, the dropping point reaches the expected value (SH / T0368-923) after the oil is pressed three times after the refining, but the working cone penetration does not reach the expected value; as a comparison, using Example 1, the oil is pressed three times after the refining, and the working cone penetration and dropping point data meet the technical index requirements of the national standard for No. 3 calcium-sodium based grease, but the finished product has a rough appearance and a low dropping point.
[0059] The dropping point and cone penetration of the two-component fat material were tested. The test plan and main analysis data are shown in Table 2.
[0060]
[0061] After the refining of Comparative Example 7, the temperature dropped to 80-90°C, and the oil was pressed 3 times. The working cone penetration did not reach the expected value, which was the worst among all the schemes. Similarly, in Comparative Example 8, the cone penetration changed too much after working 10,000 times, and the shear stability of the grease was poor. On the contrary, when using Example 2 and Comparative Example 6, the grease had a certain shear stability, especially Example 2, the calcium-sodium based grease had a delicate appearance, and the system had the best high temperature performance.
[0062] The dropping point and cone penetration of the three-component fat material were tested. The test plan and main analysis data are shown in Table 3.
[0063]
[0064] After the introduction of stearic acid, the shear stability and high temperature performance of the grease are improved. With the increase of its proportion, the high temperature performance of the calcium-sodium based grease shows a trend of first increasing and then decreasing, while the shear stability shows a trend of continuous strengthening. Comprehensively considered, Example 3 is the preferred process formula of the present invention. The comprehensive performance test is carried out, and the results are shown in Table 4.
[0065]
[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A calcium-sodium based grease, characterized in that: The invention comprises, by weight: 70-95 parts of base oil and 5-30 parts of thickener, wherein the thickener is prepared by saponification reaction of alkali and fat material, the alkali comprises sodium hydroxide and calcium hydroxide, the fat material comprises tallow, palmitoleic acid and stearic acid; the mass ratio of tallow, palmitoleic acid and stearic acid is 1:1:1-8:1:3; the mass ratio of sodium hydroxide to calcium hydroxide is 8-20:1-5; the base oil is 500SN.
2. The calcium-sodium based grease according to claim 1, characterized in that: The mass ratio of tallow, palmitic acid and stearic acid is 7:1:
2.
3. The calcium-sodium based grease according to claim 1, characterized in that: The mass ratio of the sodium hydroxide to the calcium hydroxide is 13:
3.
4. The calcium-sodium based grease according to claim 1, characterized in that: The base oil has a kinematic viscosity of 90 to 107 mm at 40°C. 2 / s, viscosity index not less than 95, pour point not less than -18℃.
5. The calcium-sodium based grease according to claim 4, characterized in that: The calcium-sodium based grease is composed of a base oil and a thickener, with the base oil accounting for 75-90% and the thickener accounting for 10-25% based on the total mass of the grease composition.
6. The calcium-sodium based grease according to claim 5, characterized in that: The calcium-sodium based grease is composed of a base oil and a thickener, with 85-90% of the base oil and 10-15% of the thickener based on the total mass of the grease composition.
7. The method for preparing the calcium-sodium based grease according to any one of claims 1 to 6, characterized in that: include: The mixed solution of base oil and fat material is mixed with the mixed aqueous solution of sodium hydroxide and calcium hydroxide, subjected to saponification reaction, heated, subjected to constant temperature treatment, thickened into fat and pressed.
8. The method for preparing the calcium-sodium based grease according to claim 7, characterized in that: The saponification reaction is a two-stage saponification reaction; the temperature of the first stage is 105-110° C., the reaction time is 50-70 min, and the temperature of the second stage is 110-115° C., the reaction time is 110-130 min.
9. The method for preparing the calcium-sodium based grease according to claim 7, characterized in that: After the saponification reaction is completed, the temperature is raised to 205-215° C. and the temperature is kept constant for 5-10 minutes.
10. The method for preparing the calcium-sodium based grease according to any one of claims 7 to 9, characterized in that: The thickening and fat-forming process includes mixing the material treated at a constant temperature with the quenching oil, reducing the temperature to 170-175° C., further reducing the temperature to 130° C., adding the rear adjustment oil, and stirring.