A high-strength aluminum alloy wire and its preparation method and application

By adjusting the elemental composition and preparation process of aluminum alloy wires, the problems of brittleness and insufficient conductivity of high magnesium alloy materials are solved, and aluminum alloy wires with high strength and good conductivity are achieved, which are suitable for pre-twisted wire materials for power fittings and are highly efficient. , low-cost production characteristics.

CN116219236BActive Publication Date: 2024-10-22JIANGSU ZHONGTIAN TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310210646.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-02
Publication Date
2024-10-22
Estimated Expiration
2043-03-02

AI Technical Summary

Technical Problem

Existing high-magnesium alloy pre-twisted wire materials have high strength but are brittle and have poor electrical conductivity. They are difficult to process and difficult to achieve mass production.

Method used

Using high-strength aluminum alloy wire, by adjusting the element composition and preparation process, including smelting, furnace refining, grain refinement, online refining, continuous casting and rolling, solution quenching, drawing and aging treatment, we prepare high-strength aluminum wire rods. and aluminum alloy wire with good electrical conductivity.

Benefits of technology

It has realized the mass and low-cost production of high-strength aluminum alloy wires with tensile strength ≥400MPa, elongation ≥3%, and electrical conductivity ≥50%IACS, overcoming the problems of brittleness and insufficient conductivity of high-magnesium alloys.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a high-strength aluminum alloy wire and its preparation method and application. Taking the total weight of the high-strength aluminum alloy wire as 100%, it includes the following elemental composition: Mg0.5-0.8%, Si0.4-0.6%, Fe0.15-0.3%, Cu0.1-0.3%, Zr0.05-0.15%, Cr0.1-0.3, Mn0.02-0.1%, Ti0.01-0.03%, and the balance is Al and impurity elements. The preparation method of the aluminum alloy wire includes: smelting, furnace refining, grain refinement, online refining, continuous casting and rolling, solution quenching, drawing, and aging treatment to obtain the high-strength aluminum alloy wire. The high-strength aluminum alloy wire provided by the present invention has high strength and good electrical conductivity, and can be used as a pre-twisted wire material for electric power hardware. The preparation method thereof has the advantages of simple process, high efficiency, and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a high-strength aluminum alloy wire and a preparation method and application thereof, in particular to a high-strength aluminum alloy pre-twisted wire for electric power fittings and a preparation method thereof, belonging to the technical field of aluminum alloys. Background Art

[0002] As a kind of power fittings, pre-twisted wire is widely used in the construction and installation of overhead power transmission line conductors. As a connection material for connecting and fixing conductors, the mechanical properties of pre-twisted wire directly determine the reliability of overhead conductor connection and the safety of overhead power transmission lines. Therefore, it must have high strength and certain conductivity.

[0003] At present, pre-twisted wires are mostly made of high-magnesium alloys. Although they have high strength, they are brittle and have poor conductivity, and the processing and preparation process is difficult. Specifically, the strength of high-magnesium mechanical alloy pre-twisted wires can reach 400MPa, but the magnesium element is easily burned during the smelting process, and the smelting process is difficult to control. In addition, high-magnesium alloys are very hard and brittle, making them difficult to roll and draw. They have high requirements for equipment and processes, and are difficult to achieve mass production.

[0004] Therefore, developing new pre-twisted wire materials and preparation processes has become one of the urgent problems to be solved in this field. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a high-strength aluminum alloy wire and its preparation method and application. The high-strength aluminum alloy wire provided by the present invention has high strength and good conductivity, and its preparation method has the advantages of simple process and high efficiency.

[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a high-strength aluminum alloy wire, which comprises the following element composition based on the total weight of the high-strength aluminum alloy wire as 100%: Mg 0.5-0.8%, Si 0.4-0.6%, Fe 0.15-0.3%, Cu 0.1-0.3%, Zr 0.05-0.15%, Cr 0.1-0.3, Mn 0.02-0.1%, Ti 0.01-0.03%, and the balance is Al and unavoidable impurity elements.

[0007] According to a specific embodiment of the present invention, preferably, based on the total weight of the high-strength aluminum alloy wire as 100%, it includes the following element composition: Mg 0.6-0.8%, Si 0.5-0.6%, Fe 0.15-0.3%, Cu 0.2-0.3%, Zr 0.1-0.15%, Cr 0.15-0.25, Mn 0.05-0.1%, Ti 0.012-0.02%, and the balance is Al and unavoidable impurity elements.

[0008] In the above-mentioned high-strength aluminum alloy wire, preferably, based on the total weight of the high-strength aluminum alloy wire as 100%, the content of a single impurity element in its elemental composition is ≤0.05%, and the total content of impurity elements is ≤0.15%.

[0009] According to a specific embodiment of the present invention, preferably, the high-strength aluminum alloy wire is prepared by at least the following steps: according to the elemental composition and weight percentage of the high-strength aluminum alloy wire, the raw material is subjected to at least the steps of smelting, furnace refining, grain refinement, online refining, continuous casting and rolling, solution quenching, drawing, aging treatment, etc., to prepare the high-strength aluminum alloy wire.

[0010] In the above-mentioned high-strength aluminum alloy wire, preferably, in the preparation step of the high-strength aluminum alloy wire, the raw materials used include aluminum ingots, magnesium ingots, silicon agent, iron agent, aluminum-titanium alloy, aluminum-zirconium alloy, aluminum-copper alloy, aluminum-chromium alloy and aluminum-manganese alloy.

[0011] In the above-mentioned high-strength aluminum alloy wire, preferably, in the preparation step of the high-strength aluminum alloy wire, the furnace refining includes: refining the smelted melt at 740-750°C by passing a mixed gas of argon and chlorine for 10-15 minutes; then skimming the melt, and then adjusting the temperature of the melt to 710-720°C and standing for 30-40 minutes.

[0012] In the above-mentioned high-strength aluminum alloy wire, preferably, in the preparation step of the high-strength aluminum alloy wire, the grain refining includes: adding a refiner to the melt after refining in the furnace for grain refining. More preferably, the refiner includes aluminum titanium boron rod, and the addition amount of the refiner is 0.05-0.15% based on the total mass of the melt as 100%.

[0013] In the above-mentioned high-strength aluminum alloy wire, preferably, in the preparation step of the high-strength aluminum alloy wire, the online refining includes: using a rotary spray degassing box to degas the melt after adding the refiner online, and using a double-stage foam ceramic filter plate to filter the melt after online degassing online, so as to further improve the cleanliness of the melt. Wherein, after adding the refiner, it can be evenly dispersed by the stirring action of the rotor of the rotary spray degassing box. More preferably, the degassing medium of the rotary spray degassing box is high-purity nitrogen, and the hydrogen content in the melt can be made less than 0.15mL / 100g after online degassing. More preferably, the porosity of the double-stage foam ceramic filter plate is 30 / 50PPI. The double-stage foam ceramic filter plate is a two-layer foam ceramic filter plate, the first layer of the filter plate has a larger pore size (30PPI), mainly filtering large-sized inclusions, and the second layer of the filter plate has a smaller pore size (50PPI), filtering small-sized inclusions, and the double-stage filtration has the advantages of a wider filtration range and higher filtration accuracy.

[0014] In the above-mentioned high-strength aluminum alloy wire, preferably, in the preparation step of the high-strength aluminum alloy wire, the continuous casting and rolling includes: pouring the melt after online refining into a wheel-type crystallizer for continuous casting to form a cast billet; the cast billet enters a continuous rolling mill for continuous rolling to obtain an aluminum alloy rod. More preferably, the cross-sectional area of ​​the cast billet is 2400mm 2 , the casting temperature is 705-715°C, the casting speed is 8-12m / min, the cooling water temperature is 15-40°C, and the cooling water pressure is 0.35-0.5MPa. More preferably, the casting billet enters the continuous rolling mill and the rolling temperature is controlled to be 500-520°C. The continuous rolling mill adopts a three-roll mill to obtain an aluminum alloy rod after rolling. More preferably, the diameter of the aluminum alloy rod is 9-10mm. More preferably, the continuous rolling mill adopts a 15-frame three-roll mill. Among them, the equipment used for continuous casting and continuous rolling are all equipment in the prior art.

[0015] In the above-mentioned high-strength aluminum alloy wire, preferably, in the preparation step of the high-strength aluminum alloy wire, the solid solution quenching includes: performing solid solution quenching treatment on the aluminum alloy rod, keeping the temperature at 450-530°C for 2-3 hours for solid solution treatment, and then quenching and cooling. More preferably, the quenching and cooling is performed in a water tank with a water temperature of 20-30°C.

[0016] In the above-mentioned high-strength aluminum alloy wire, preferably, in the preparation step of the high-strength aluminum alloy wire, the drawing includes: drawing the aluminum alloy rod after solid solution quenching treatment to obtain the aluminum alloy wire. More preferably, the diameter of the aluminum alloy wire is 2.5 to 5.0 mm. More preferably, the drawing can be carried out using a sliding wire drawing machine, the drawing die can be a tungsten steel die, the drawing speed is 8 to 10 m / s, and the final drawing dimensional accuracy is controlled within ±0.03 mm.

[0017] In the above-mentioned high-strength aluminum alloy wire, preferably, in the preparation step of the high-strength aluminum alloy wire, the aging treatment comprises: performing aging treatment on the drawn aluminum alloy wire, the aging treatment temperature is 140-180° C., and the insulation time is 6-15 hours to obtain the high-strength aluminum alloy wire.

[0018] According to a specific embodiment of the present invention, preferably, the high-strength aluminum alloy wire has a tensile strength of ≥400 MPa, an elongation of ≥3%, and a conductivity of ≥50% IACS.

[0019] The second aspect of the present invention provides a method for preparing the above-mentioned high-strength aluminum alloy wire, which comprises the following steps: according to the element composition and weight percentage of the high-strength aluminum alloy wire, subjecting the raw materials to at least smelting, furnace refining, grain refining, online refining, continuous casting and rolling, solution quenching, drawing, aging treatment and other steps to obtain the high-strength aluminum alloy wire;

[0020] The continuous casting and rolling process includes: pouring the melt after online refining into a wheel-type crystallizer for continuous casting to form a cast billet; the cast billet enters a continuous rolling unit for continuous rolling to obtain an aluminum alloy rod;

[0021] The solution quenching comprises: performing solution quenching treatment on the aluminum alloy rod material, maintaining the temperature at 450 to 530° C. for 2 to 3 hours for solution treatment, and then quenching and cooling;

[0022] The aging treatment comprises: performing aging treatment on the drawn aluminum alloy wire, the aging treatment temperature is 140-180° C., and the heat preservation time is 6-15 hours.

[0023] In the above-mentioned preparation method, preferably, the raw materials used include aluminum ingots, magnesium ingots, silicon agent, iron agent, aluminum-titanium alloy, aluminum-zirconium alloy, aluminum-copper alloy, aluminum-chromium alloy and aluminum-manganese alloy.

[0024] In the above-mentioned preparation method, preferably, the furnace refining comprises: refining the smelted melt in a furnace at 740-750°C by introducing a mixed gas of argon and chlorine for 10-15 minutes; then skimming the melt, adjusting the temperature of the melt to 710-720°C, and standing for 30-40 minutes.

[0025] In the above preparation method, preferably, the grain refining comprises: adding a refiner to the melt after refining in the furnace for grain refining. More preferably, the refiner comprises aluminum titanium boron rods, and the addition amount of the refiner is 0.05-0.15% based on the total mass of the melt as 100%.

[0026] In the above-mentioned preparation method, preferably, the online refining includes: using a rotary spray degassing box to degas the melt after adding the refiner online, and using a two-stage foam ceramic filter plate to filter the melt after online degassing online, so as to further improve the cleanliness of the melt. After adding the refiner, it can be evenly dispersed by the stirring action of the rotor of the rotary spray degassing box. More preferably, the degassing medium of the rotary spray degassing box is high-purity nitrogen, and the hydrogen content in the melt can be reduced to <0.15mL / 100g after online degassing. More preferably, the porosity of the two-stage foam ceramic filter plate is 30 / 50PPI.

[0027] In the above-mentioned preparation method, preferably, the cross-sectional area of ​​the ingot formed after continuous casting is 2400mm 2 The casting temperature is 705-715°C, the casting speed is 8-12m / min, the cooling water temperature is 15-40°C, and the cooling water pressure is 0.35-0.5MPa.

[0028] In the above-mentioned preparation method, preferably, the temperature of the cast billet entering the continuous rolling mill is controlled to be 500-520°C, and the continuous rolling mill adopts a three-roll rolling mill to obtain the aluminum alloy rod after rolling. More preferably, the diameter of the aluminum alloy rod is 9-10 mm. Particularly preferably, the continuous rolling mill adopts a 15-frame three-roll rolling mill.

[0029] In the above preparation method, preferably, the solution quenching is performed by quenching and cooling in a water tank with a water temperature of 20 to 30°C.

[0030] In the above-mentioned preparation method, preferably, the drawing includes: drawing the aluminum alloy rod after solid solution quenching treatment to obtain an aluminum alloy wire. More preferably, the diameter of the aluminum alloy wire is 2.5-5.0 mm. More preferably, the drawing can be carried out using a sliding wire drawing machine, the drawing die can be a tungsten steel die, the drawing speed is 8-10 m / s, and the final drawing dimensional accuracy is controlled within ±0.03 mm.

[0031] A third aspect of the present invention provides the use of the above-mentioned high-strength aluminum alloy wire as a pre-twisted wire material for electric power fittings.

[0032] The present invention provides a high-strength aluminum alloy wire and a preparation method and application thereof. The present invention adjusts the element composition of the aluminum alloy wire and adopts the continuous casting and rolling method for production, thereby overcoming the disadvantage that the high-magnesium mechanical alloy wire is difficult to roll and draw due to its high hardness, thereby realizing batch production of high-strength aluminum alloy wire at low cost; at the same time, by solid solution treatment of the aluminum alloy rod, elements such as Mg, Si, and Cu are fully dissolved back into the aluminum-based solid solution, and a supersaturated state is reached through quenching, providing sufficient conditions for subsequent maximum aging precipitation strengthening, so that Zr is used as Al 3 Zr dispersed phase precipitates to improve high temperature strength; and, the aluminum alloy wire after drawing is subjected to aging treatment, so that the dissolved elements such as Mg, Si, and Cu are fully precipitated as metastable dispersed phases. With the combined effect of work hardening and dispersed phase precipitation strengthening, the wire strength is greatly improved, overcoming the shortcomings of 5××× high magnesium alloy that only relies on work hardening to improve strength and drawing processing is difficult, and at the same time, the electrical conductivity of the wire is improved to a certain extent. Therefore, through the elemental composition and preparation process of the aluminum alloy wire of the present invention, the tensile strength of the prepared aluminum alloy wire is ≥400MPa, the elongation is ≥3%, and the conductivity is ≥50%IACS. The high-strength aluminum alloy wire of the present invention can be used as a pre-twisted wire material for power hardware for the installation of overhead power transmission lines. In addition, the preparation method of the present invention has the advantages of simple process, high efficiency, and low cost. DETAILED DESCRIPTION

[0033] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.

[0034] According to a specific embodiment of the present invention, preferably, the high-strength aluminum alloy wire provided by the present invention comprises the following element composition by weight percentage: Mg 0.5-0.8%, Si 0.4-0.6%, Fe 0.15-0.3%, Cu 0.1-0.3%, Zr 0.05-0.15%, Cr 0.1-0.3, Mn 0.02-0.1%, Ti 0.01-0.03%, the balance being Al and unavoidable impurity elements, wherein the content of a single impurity element is ≤0.05%, and the total content of impurity elements is ≤0.15%;

[0035] The high-strength aluminum alloy wire is prepared by the following steps:

[0036] (1) Melting

[0037] According to the element composition and weight percentage of the high-strength aluminum alloy wire, an aluminum ingot, a silicon agent, an iron agent, an aluminum-titanium alloy, an aluminum-zirconium alloy, an aluminum-copper alloy, an aluminum-chromium alloy and an aluminum-manganese alloy are added to a smelting furnace, heated and melted to obtain molten aluminum liquid; then a magnesium ingot is added to the aluminum liquid, and the molten melt is fully stirred;

[0038] (2) Furnace refining

[0039] The melt in the smelting furnace is transferred to a tilting holding furnace, the electromagnetic stirring device at the bottom of the furnace is turned on to stir the melt, the melt temperature is adjusted to 740-750°C, a mixed gas of argon and chlorine is introduced for furnace refining, the furnace refining time is 10-15 minutes, the hydrogen content in the melt is controlled to be less than 0.35mL / 100g, the surface scum is scraped off, and then the melt temperature is readjusted to 710-720°C and left to stand for 30-40 minutes;

[0040] (3) Grain refinement

[0041] In the process of pouring the melt refined in the furnace into the wheel crystallizer through the launder for continuous casting, aluminum titanium boron rods are added online in the launder to refine the melt grains, and the addition amount of the aluminum titanium boron rods is 0.05-0.15% based on the total mass of the melt as 100%;

[0042] (4) Online refining

[0043] Afterwards, the melt in the flow trough is refined online, and the online refining includes online degassing and online filtration; a rotary spray degassing box is used to degas the melt after adding the aluminum titanium boron rods, and the dissolved aluminum titanium boron rods are evenly dispersed by the stirring action of the rotor of the rotary spray degassing box, and high-purity nitrogen is used as the degassing medium. After online degassing, the hydrogen content in the melt can be less than 0.15mL / 100g; a double-stage foam ceramic filter plate is used to filter the melt after online degassing. The porosity of the double-stage foam ceramic filter plate is 30 / 50PPI, which can effectively remove 5-10μm inclusion particles, thereby further improving the cleanliness of the melt;

[0044] (5) Continuous casting and rolling

[0045] The melt after online refining is poured into a wheel crystallizer of a continuous casting equipment for continuous casting, with a casting temperature of 705-715°C, a casting speed of 8-12 m / min, a cooling water temperature of 15-40°C, and a cooling water pressure of 0.35-0.5 MPa to form a cast billet with a cross-sectional area of ​​2400 mm 2; After the ingot comes out of the crystallization wheel, it enters the continuous rolling mill for continuous rolling. The continuous rolling mill adopts a 15-frame three-roller rolling mill, and the rolling temperature is controlled to be 500-520°C. After rolling, an aluminum alloy rod is obtained. The diameter of the aluminum alloy rod is 9-10 mm. The aluminum alloy rod is cooled by online cooling water and then coiled;

[0046] (6) Solution quenching

[0047] The aluminum alloy rod after coiling is subjected to solution quenching treatment, and the solution treatment is carried out at a temperature of 450-530°C for 2-3 hours, and then quenched and cooled in a water tank at a water temperature of 20-30°C;

[0048] (7) Drawing

[0049] Drawing the aluminum alloy rod after solid solution quenching treatment on a sliding wire drawing machine, using a tungsten steel die as the drawing die, with a drawing speed of 8 to 10 m / s, and controlling the final drawing dimensional accuracy within ±0.03 mm to obtain an aluminum alloy wire having a diameter of 2.5 to 5.0 mm;

[0050] (8) Time limit

[0051] The drawn aluminum alloy wire is subjected to aging treatment, wherein the aging treatment temperature is 140 to 180° C. and the insulation time is 6 to 15 hours to obtain the high-strength aluminum alloy wire.

[0052] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0053] Example 1

[0054] This embodiment provides a high-strength aluminum alloy wire, which is prepared by the following steps:

[0055] Step 1: adding aluminum ingots, silicon agent, iron agent, aluminum-titanium alloy, aluminum-zirconium alloy, aluminum-copper alloy, aluminum-chromium alloy and aluminum-manganese alloy into a smelting furnace, heating and melting, and then adding magnesium ingots into the aluminum liquid to melt and stir;

[0056] Step 2: Transfer the melt in the smelting furnace to a tilting holding furnace, turn on the electromagnetic stirring device at the bottom of the furnace to stir the melt, adjust the melt temperature to 740°C, introduce a mixed gas of argon and chlorine (the volume ratio of argon to chlorine is 95:5) for furnace refining for 10 minutes, control the hydrogen content in the melt to less than 0.35mL / 100g, scrape off the surface scum, and then readjust the melt temperature to 715°C and let it stand for 30 minutes;

[0057] Step 3: After the casting starts, aluminum titanium boron rods are added online in the flow channel to refine the melt grains. The addition amount of aluminum titanium boron rods is 0.055% based on the total mass of the melt as 100%;

[0058] Step 4: online refining of the melt in the convection trough, online degassing of the melt after adding the aluminum titanium boron rod using a rotary spray degassing box, and evenly dispersing the dissolved aluminum titanium boron rod by means of the stirring action of the rotor of the rotary spray degassing box, the degassing box uses high-purity nitrogen as the degassing medium, and the hydrogen content in the melt is less than 0.15mL / 100g after online degassing; online filtering of the melt after online degassing using a double-stage foam ceramic filter plate, the porosity of the double-stage foam ceramic filter plate is 30 / 50PPI, and the inclusion particles of 5 to 10μm are effectively removed;

[0059] Step 5: The melt after online refining is poured into a wheel-type crystallizer for continuous casting. The casting temperature is 710°C, the casting speed is 10m / min, the cooling water temperature is 15°C, the cooling water pressure is 0.38MPa, and the cross-sectional area of ​​the ingot is 2400mm 2 ; After the ingot comes out of the crystallization wheel, it enters the continuous rolling unit for continuous rolling. The continuous rolling unit adopts a 15-frame three-roller rolling mill, and the rolling temperature is controlled to be 510°C to obtain an aluminum alloy rod with a diameter of 9.5mm. The aluminum alloy rod is cooled by online cooling water and then coiled;

[0060] Step 6: The aluminum alloy rod is subjected to solution quenching treatment at 500°C for 3 hours, and then quenched in a water tank at a water temperature of 20-30°C.

[0061] Step 7: Drawing the aluminum alloy rod after solution quenching treatment on a sliding wire drawing machine, the drawing die adopts a tungsten steel die, the drawing speed is 9m / s, and the final drawing dimensional accuracy is controlled within ±0.03mm to obtain an aluminum alloy wire, the diameter of which is 3.5mm;

[0062] Step eight: performing aging treatment on the aluminum alloy wire, wherein the aging temperature is 160° C. and the insulation time is 8 hours to obtain the high-strength aluminum alloy wire.

[0063] After analysis and detection, the element composition of the high-strength aluminum alloy wire provided in this embodiment is: in weight percentage, Mg0.68%, Si0.55%, Fe 0.21%, Cu 0.23%, Zr0.12%, Cr0.25%, Mn0.05%, Ti0.013%, and the rest is Al and other inevitable impurity elements, among which the content of a single impurity element is ≤0.05%, and the total content of impurity elements is ≤0.15%.

[0064] The high-strength aluminum alloy wire has a tensile strength of 412 MPa, an elongation of 3.8%, and a conductivity of 50.78% IACS. The high-strength aluminum alloy wire can be used as a pre-twisted wire for electric power fittings.

[0065] Example 2

[0066] This embodiment provides a high-strength aluminum alloy wire, which is prepared by the following steps:

[0067] Step 1: adding aluminum ingots, silicon agent, iron agent, aluminum-titanium alloy, aluminum-zirconium alloy, aluminum-copper alloy, aluminum-chromium alloy and aluminum-manganese alloy into a smelting furnace, heating and melting, and then adding magnesium ingots into the aluminum liquid to melt and stir;

[0068] Step 2: Transfer the melt in the smelting furnace to a tilting holding furnace, turn on the electromagnetic stirring device at the bottom of the furnace to stir the melt, adjust the melt temperature to 740°C, introduce a mixed gas of argon and chlorine (the volume ratio of argon to chlorine is 95:5) for furnace refining for 10 minutes, control the hydrogen content in the melt to less than 0.35mL / 100g, scrape off the surface scum, and then readjust the melt temperature to 720°C and let it stand for 30 minutes;

[0069] Step 3: After the casting starts, aluminum titanium boron rods are added online in the flow channel to refine the melt grains. The addition amount of aluminum titanium boron rods is 0.062% based on the total mass of the melt as 100%;

[0070] Step 4: online refining of the melt in the convection trough, online degassing of the melt after adding the aluminum titanium boron rod using a rotary spray degassing box, and evenly dispersing the dissolved aluminum titanium boron rod by means of the stirring action of the rotor of the rotary spray degassing box, the degassing box uses high-purity nitrogen as the degassing medium, and the hydrogen content in the melt is less than 0.15mL / 100g after online degassing; online filtering of the melt after online degassing using a double-stage foam ceramic filter plate, the porosity of the double-stage foam ceramic filter plate is 30 / 50PPI, and the inclusion particles of 5 to 10μm are effectively removed;

[0071] Step 5: The melt after online refining is poured into a wheel-type crystallizer for continuous casting. The casting temperature is 710°C, the casting speed is 10m / min, the cooling water temperature is 25°C, the cooling water pressure is 0.35MPa, and the cross-sectional area of ​​the ingot is 2400mm 2 ; After the ingot comes out of the crystallization wheel, it enters the continuous rolling unit for continuous rolling. The continuous rolling unit adopts a 15-frame three-roller rolling mill, and the rolling temperature is controlled to be 510°C to obtain an aluminum alloy rod with a diameter of 9.5mm. The aluminum alloy rod is cooled by online cooling water and then coiled;

[0072] Step 6: Solution quench the aluminum alloy rod at 520°C for 3 hours, and then quench and cool in a water tank at a water temperature of 20-30°C.

[0073] Step 7: Drawing the aluminum alloy rod after solution quenching treatment on a sliding wire drawing machine, the drawing die adopts a tungsten steel die, the drawing speed is 10m / s, and the final drawing dimensional accuracy is controlled within ±0.03mm to obtain an aluminum alloy wire, the diameter of which is 3.0mm;

[0074] Step eight: performing aging treatment on the aluminum alloy wire, the aging temperature is 165° C., and the insulation time is 9 hours to obtain the high-strength aluminum alloy wire.

[0075] After analysis and detection, the element composition of the high-strength aluminum alloy wire provided in this embodiment is: by weight percentage, Mg 0.73%, Si 0.55%, Fe 0.19%, Cu 0.27%, Zr 0.14%, Cr 0.15%, Mn 0.08%, Ti0.018%, and the rest is Al and other inevitable impurity elements, wherein the content of a single impurity element is ≤0.05%, and the total content of impurity elements is ≤0.15%.

[0076] The high-strength aluminum alloy wire has a tensile strength of 428 MPa, an elongation of 3.4%, and a conductivity of 50.21% IACS. The high-strength aluminum alloy wire can be used as a pre-twisted wire for power fittings.

[0077] Comparative Example 1

[0078] This comparative example provides an aluminum alloy wire, which is prepared by the following steps:

[0079] Step 1: Add aluminum ingots, silicon agent, iron agent, aluminum-titanium alloy, and aluminum-copper alloy into a smelting furnace and heat to melt, then add magnesium ingots into the aluminum liquid to melt and stir;

[0080] Step 2: Transfer the melt in the smelting furnace to a tilting holding furnace, turn on the electromagnetic stirring device at the bottom of the furnace to stir the melt, adjust the melt temperature to 740°C, introduce a mixed gas of argon and chlorine (the volume ratio of argon to chlorine is 95:5) for furnace refining for 10 minutes, control the hydrogen content in the melt to less than 0.35mL / 100g, scrape off the surface scum, and then readjust the melt temperature to 715°C and let it stand for 30 minutes;

[0081] Step 3: After the casting starts, aluminum titanium boron rods are added online in the flow channel to refine the melt grains. The addition amount of aluminum titanium boron rods is 0.05% based on the total mass of the melt as 100%;

[0082] Step 4: online refining of the melt in the convection trough, online degassing of the melt after adding the aluminum titanium boron rod using a rotary spray degassing box, and evenly dispersing the dissolved aluminum titanium boron rod by means of the stirring action of the rotor of the rotary spray degassing box, the degassing box uses high-purity nitrogen as the degassing medium, and the hydrogen content in the melt is less than 0.15mL / 100g after online degassing; online filtering of the melt after online degassing using a double-stage foam ceramic filter plate, the porosity of the double-stage foam ceramic filter plate is 30 / 50PPI, and the inclusion particles of 5 to 10μm are effectively removed;

[0083] Step 5: The melt after online refining is poured into a wheel-type crystallizer for continuous casting. The casting temperature is 710°C, the casting speed is 10m / min, the cooling water temperature is 15°C, the cooling water pressure is 0.38MPa, and the cross-sectional area of ​​the ingot is 2400mm 2 ; After the ingot comes out of the crystallization wheel, it enters the continuous rolling unit for continuous rolling. The continuous rolling unit adopts a 15-frame three-roller rolling mill, and the rolling temperature is controlled to be 510°C to obtain an aluminum alloy rod with a diameter of 9.5mm. The aluminum alloy rod is cooled by online cooling water and then coiled;

[0084] Step 6: Perform aging treatment on the aluminum alloy rod, the aging temperature is 180° C., and the insulation time is 15 hours;

[0085] Step seven: Drawing the aluminum alloy rod after aging treatment on a sliding wire drawing machine, using a tungsten steel die as the drawing die, with a drawing speed of 9 m / s, and the final drawing dimensional accuracy is controlled within ±0.03 mm to obtain an aluminum alloy wire having a diameter of 3.5 mm.

[0086] After analysis and detection, the element composition of the aluminum alloy wire provided in this comparative example is: in weight percentage, Mg0.54%, Si 0.46%, Fe 0.15%, Cu 0.05%, Ti 0.01%, and the rest is Al and other inevitable impurity elements, among which the content of a single impurity element is ≤0.05%, and the total content of impurity elements is ≤0.15%.

[0087] The aluminum alloy wire has a tensile strength of 296 MPa, an elongation of 4.8%, and a conductivity of 56.5% IACS.

[0088] Comparative Example 2

[0089] This comparative example provides an aluminum alloy wire, which is prepared by the following steps:

[0090] Step 1: adding aluminum ingots, silicon agent, iron agent, aluminum-titanium alloy, aluminum-zirconium alloy, aluminum-copper alloy, aluminum-chromium alloy and aluminum-manganese alloy into a smelting furnace, heating and melting, and then adding magnesium ingots into the aluminum liquid to melt and stir;

[0091] Step 2: Transfer the melt in the smelting furnace to a tilting holding furnace, turn on the electromagnetic stirring device at the bottom of the furnace to stir the melt, adjust the melt temperature to 740°C, introduce a mixed gas of argon and chlorine (the volume ratio of argon to chlorine is 95:5) for furnace refining for 10 minutes, control the hydrogen content in the melt to less than 0.35mL / 100g, scrape off the surface scum, and then readjust the melt temperature to 720°C and let it stand for 30 minutes;

[0092] Step 3: After the casting starts, aluminum titanium boron rods are added online in the flow channel to refine the melt grains. The addition amount of aluminum titanium boron rods is 0.061% based on the total mass of the melt as 100%;

[0093] Step 4: online refining of the melt in the convection trough, online degassing of the melt after adding the aluminum titanium boron rod using a rotary spray degassing box, and evenly dispersing the dissolved aluminum titanium boron rod by means of the stirring action of the rotor of the rotary spray degassing box, the degassing box uses high-purity nitrogen as the degassing medium, and the hydrogen content in the melt is less than 0.15mL / 100g after online degassing; online filtering of the melt after online degassing using a double-stage foam ceramic filter plate, the porosity of the double-stage foam ceramic filter plate is 30 / 50PPI, and the inclusion particles of 5 to 10μm are effectively removed;

[0094] Step 5: The melt after online refining is poured into a wheel-type crystallizer for continuous casting. The casting temperature is 710°C, the casting speed is 10m / min, the cooling water temperature is 15°C, the cooling water pressure is 0.4MPa, and the cross-sectional area of ​​the ingot is 2400mm 2 ; After the ingot comes out of the crystallization wheel, it enters the continuous rolling unit for continuous rolling. The continuous rolling unit adopts a 15-frame three-roller rolling mill, and the rolling temperature is controlled to be 510°C to obtain an aluminum alloy rod with a diameter of 9.5mm. The aluminum alloy rod is cooled by online cooling water and then coiled;

[0095] Step 6: Drawing the aluminum alloy rod on a sliding wire drawing machine, the drawing die adopts a tungsten steel die, the drawing speed is 9 m / s, and the final drawing dimensional accuracy is controlled within ±0.03 mm to obtain an aluminum alloy wire, the diameter of which is 3.5 mm;

[0096] Step seven: performing aging treatment on the aluminum alloy wire, wherein the aging temperature is 160° C. and the insulation time is 8 hours to obtain the aluminum alloy wire.

[0097] After analysis and detection, the element composition of the aluminum alloy wire provided in this comparative example is: in weight percentage, Mg0.66%, Si0.52%, Fe 0.24%, Cu 0.2%, Zr 0.12%, Cr 0.25%, Mn 0.07%, Ti0.012%, and the rest is Al and other inevitable impurity elements, among which the content of a single impurity element is ≤0.05%, and the total content of impurity elements is ≤0.15%.

[0098] The aluminum alloy wire has a tensile strength of 344 MPa, an elongation of 4.6%, and a conductivity of 52.6% IACS.

[0099] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A high-strength aluminum alloy wire, which, based on the total weight of the high-strength aluminum alloy wire being 100%, comprises the following elements: composition: Mg 0.5-0.8%, Si 0.4-0.6%, Fe 0.15-0.3%, Cu 0.1-0.3%, Zr 0.05-0.15%, Cr 0.1-0.3%, Mn 0.02-0.1%, Ti 0.01-0.03%, the balance is Al and unavoidable impurity elements; The high-strength aluminum alloy wire is prepared by at least the following steps: according to the element composition and weight percentage of the high-strength aluminum alloy wire, the raw materials are subjected to at least smelting, furnace refining, grain refinement, online refining, continuous casting and rolling, solution quenching, drawing, and aging treatment to prepare the high-strength aluminum alloy wire; The continuous casting and rolling process includes: pouring the melt after online refining into a wheel-type crystallizer for continuous casting to form a cast billet; the cast billet enters a continuous rolling unit for continuous rolling to obtain an aluminum alloy rod; The solid solution quenching comprises: performing solid solution quenching treatment on the aluminum alloy rod material, maintaining the temperature at 450-530° C. for 2-3 hours for solid solution treatment, and then quenching and cooling; The aging treatment comprises: performing aging treatment on the drawn aluminum alloy wire, wherein the aging treatment temperature is 140-180° C. and the holding time is 6-15 hours; The high-strength aluminum alloy wire has a tensile strength of ≥400 MPa, an elongation of ≥3%, and a conductivity of ≥50% IACS.

2. The high-strength aluminum alloy wire according to claim 1, in, Taking the total weight of the high-strength aluminum alloy wire as 100%, the content of a single impurity element in its elemental composition is ≤0.05%, and the total content of impurity elements is ≤0.15%.

3. A method for preparing the high-strength aluminum alloy wire according to claim 1 or 2, wherein The following steps are involved: According to the element composition and weight percentage of the high-strength aluminum alloy wire, the raw materials are subjected to at least smelting, furnace refining, grain refinement, online refining, continuous casting and rolling, solution quenching, drawing, and aging treatment to prepare the high-strength aluminum alloy wire; The continuous casting and rolling process includes: pouring the melt after online refining into a wheel-type crystallizer for continuous casting to form a cast billet; the cast billet enters a continuous rolling unit for continuous rolling to obtain an aluminum alloy rod; The solid solution quenching comprises: performing solid solution quenching treatment on the aluminum alloy rod material, maintaining the temperature at 450-530° C. for 2-3 hours for solid solution treatment, and then quenching and cooling; The aging treatment comprises: performing aging treatment on the drawn aluminum alloy wire, the aging treatment temperature is 140-180° C., and the insulation time is 6-15 hours.

4. The preparation method according to claim 3, in, The furnace refining comprises: refining the melt at 740-750° C. by introducing a mixed gas of argon and chlorine for 10-15 minutes; then deslagging the melt, adjusting the temperature of the melt to 710-720° C., and standing for 30-40 minutes.

5. The preparation method according to claim 3, in, The grain refining comprises: adding a refiner to the melt after refining in the furnace to perform grain refining.

6. The preparation method according to claim 5, in, The refiner includes aluminum titanium boron rods. Based on the total mass of the melt as 100%, the added amount of the refiner is 0.05-0.15%.

7. The preparation method according to claim 3, in, The online refining comprises: using a rotary spray degassing box to perform online degassing on the melt after adding a refiner, and using a double-stage foam ceramic filter plate to perform online filtering on the melt after online degassing.

8. The preparation method according to claim 7, in, The degassing medium of the rotary spray degassing box is high-purity nitrogen, and the hydrogen content in the melt is reduced to <0.15mL / 100g through online degassing.

9. The preparation method according to claim 7, in, The double-stage foam ceramic filter plate adopts two layers of foam ceramic filter plates; the first layer of filter plates has a larger pore size and a porosity of 30PPI; the second layer of filter plates has a smaller pore size and a porosity of 50PPI.

10. The preparation method according to claim 3, in, The cross-sectional area of ​​the billet formed after continuous casting is 2400mm 2 The casting temperature is 705~715℃, the casting speed is 8~12m / min, the cooling water temperature is 15~40℃, and the cooling water pressure is 0.35~0.5MPa.

11. The preparation method according to claim 3, in, The casting billet enters the continuous rolling mill and the rolling temperature is controlled to be 500-520°C. The continuous rolling mill adopts a three-roller rolling mill to obtain aluminum alloy rods after rolling.

12. The preparation method according to claim 11, in, The diameter of the aluminum alloy rod is 9-10 mm.

13. The preparation method according to claim 11, in, The continuous rolling mill group adopts a three-roller rolling mill with 15 frames.

14. The preparation method according to claim 3, in, The solution quenching is performed by quenching in a water tank with a water temperature of 20-30°C.

15. The preparation method according to claim 3, in, The drawing comprises: drawing the aluminum alloy rod after solid solution quenching treatment to obtain an aluminum alloy wire, wherein the diameter of the aluminum alloy wire is 2.5-5.0 mm.

16. Use of the high-strength aluminum alloy wire material according to claim 1 or 2 as pre-twisted wire material for electric power fittings.