A hollow nano-silicon sphere containing titanium ion functional groups and its preparation and application

Preparation of titanium ion functionalized hollow nanosilicon spheres through potassium sulfate-induced sol-gel reaction, solving the problems of low phosphopeptide enrichment efficiency and lack of IMAC methods in existing materials, and achieving rapid and efficient phosphopeptide enrichment , with high selectivity and sensitivity.

CN116251573BActive Publication Date: 2024-11-22DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111518039.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-09
Publication Date
2024-11-22
Estimated Expiration
2041-12-09

AI Technical Summary

Technical Problem

The existing phosphopeptide enrichment materials have long and complex pores, slow mass transfer and large mass transfer resistance, resulting in low site utilization and lack of hollow nanomaterials based on IMAC method for phosphopeptide enrichment.

Method used

The hollow nanosilicon spheres containing phosphonate were prepared by potassium sulfate-induced sol-gel reaction, and then dealkylated into phosphate groups by hydrochloric acid and chelated with titanium ions to form titanium ion functional hollow nanosilicon spheres. , used for rapid, high sensitivity and high selectivity enrichment of phosphopeptides.

Benefits of technology

The rapid enrichment of phosphopeptides was achieved, and the enrichment efficiency was improved. The shell was thin and uniform, the mass transfer resistance was small, and the site utilization rate was high. The IMAC method was used for phosphopeptide enrichment for the first time, which had good specificity and selectivity. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116251573B_ABST
    Figure CN116251573B_ABST
Patent Text Reader

Abstract

The present invention relates to the preparation of hollow nano-silicon spheres containing titanium ion functional groups and their application in phosphopeptide enrichment. Specifically, under neutral conditions, a sol-gel reaction is adopted, diethylphosphoethyltriethoxysilane and tetramethoxysilane are used as hydrolysis and polycondensation silicon source monomers, F127 is used as a surfactant, mesitylene is used as a swelling agent, potassium sulfate is used as an auxiliary agent, and water is used as a solvent to prepare hollow nano-silicon spheres containing phosphonates, and the phosphonates in the hollow nano-silicon spheres can be dealkylated to phosphoric acid functional groups after acidification with hydrochloric acid, and further chelated with the phosphoric acid functional groups by titanium ions to obtain a material that can be used as a fixed metal ion affinity chromatography stationary phase for rapid, highly sensitive and highly selective enrichment of phosphopeptides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a hollow nano-silicon sphere containing titanium ion functional groups prepared by sol-gel reaction under neutral conditions and its application in phosphopeptide enrichment. Specifically, hollow nano-silicon spheres containing phosphonates are first prepared by sol-gel reaction induced by potassium sulfate, and the phosphonates in the hollow nano-silicon spheres are dealkylated to phosphoric acid groups after acidification with hydrochloric acid, and then chelated with titanium ions, and finally hollow nano-silicon spheres functionalized with titanium ions that can be used for phosphopeptide enrichment in complex biological samples are obtained. Background Art

[0002] Protein phosphorylation is one of the most widely studied protein post-translational modifications. More than 293,000 phosphorylation modification sites have been found, accounting for 65% of the modification types (Reference 1, Hornbeck et al., 15 years of integrating post-translationally modified sites, diseasevariants and isoforms. Nucleic Acids Res. 2019;47(D1):D433-D41.). Studies have also found that protein phosphorylation plays a key role in an increasing number of biological processes and diseases, such as liquid-liquid phase separation (Reference 2, Alberti et al., Considerations and Challenges in Studying Liquid-Liquid Phase Separation and Biomolecular Condensates. Cell. 2019; 176(3): 419-34.), small ubiquitin-like modification (Reference 3, Hendriks et al., Site-specific mapping of the human SUMO proteome reveals co-modification with phosphorylation. Nat Struct Mol Biol. 2017; 24(3): 325-36.) and cancer progression (Reference 4, Su et al., CD10(+)GPR77(+)Cancer-Associated Fibroblasts Promote Cancer Formation and Chemoresistance by Sustaining Cancer Stemness. Cell. 2018; 172(4): 841-56e16.). Therefore, it is of great significance to continuously develop new methods to identify phosphorylation. Mass spectrometry-based technologies have made it possible to accurately and deeply characterize peptides and proteins, greatly promoting the development of peptidomics and proteomics. However, since a large number of highly abundant interfering proteins and non-phosphopeptides can suppress the signals of phosphopeptides, it is still a challenge to identify substoichiometric phosphopeptides, which makes the separation and enrichment of phosphopeptides before mass spectrometry analysis a key step.

[0003] Immobilized metal ion affinity chromatography (IMAC) and metal oxide affinity chromatography (MOAC) are two commonly used phosphopeptide enrichment methods that have emerged in recent years (Reference 5, Xu et al., Hydrophililic polydopamine-derived mesoporous channels for loading Ti(IV)ions for salivary phosphoproteomeresearch.Analytica Chimica Acta.2021;1146:53-60.). Among them, porous materials have been widely developed as IMAC stationary phase materials due to their advantages such as high specific surface area and adjustable pore size. Many three-dimensional materials with three-dimensional interconnected pore structures or two-dimensional hexagonal pore structures have been designed and used to enrich phosphopeptides (Reference 6, Wang et al., Phosphonic Acid Functionalized Periodic Mesoporous Organosilicas and Their Potential Applications in Selective Enrichment of Phosphopeptides. The Journal of Physical Chemistry C. 2009; 113(4): 1359-66., Reference 7, Guo et al., TiO2-functionalized mesoporous materials for sensitive analysis of multi-phosphopeptides. Science China Chemistry. 2011; 54(8): 1327., Reference 8, Wang et.al., Titanium(IV)ion-modified covalent organic frameworks for specific enrichmentof phosphopeptides. Talanta. 2017; 166: 133-40.). In general, these materials have long and complex pores, slow mass transfer, large mass transfer resistance, and may result in low site utilization.In previous reports, the loading time of phosphopeptides is generally more than 15 minutes, and the elution time is generally more than 10 minutes (Reference 8, Luo et al., Boronic Acid-Functionalized Magnetic Metal–Organic Frameworks via a Dual-Lig and Strategy for Highly Efficient Enrichment of Phosphopeptides and Glycopeptides. ACS Sustainable Chemistry & Engineering. 2019; 7(6): 6043-52., Reference 9, Li et al., Guanidyl-Functionalized Magnetic Bimetallic MOF Nanocomposites Developed for Selective Enrichment of Phosphopeptides. ACS Sustainable Chemistry & Engineering. 2020; 8(44): 16422-9., Reference 10, Xiong et al., Facile synthesis of guanidyl-based magnetic ionic covalent organic framework composites for selective enrichment of phosphopeptides. Analytical Chemistry. Chimica Acta. 2020; 1099: 103-10.). Therefore, developing a material with a large specific surface area and simple pores is of great significance for achieving rapid enrichment of phosphopeptides, especially the enrichment of unstable phosphopeptides.Hollow nanostructures are widely used in catalysts, reactors and drug delivery systems due to their advantages such as large specific surface area, clearly positioned active sites, independent cavity structure and adjustable mass transfer rate (Reference 11, Zhu et al., Functionalization of Hollow Nanomaterials for Catalytic Applications: Nanoreactor Construction. Advanced Materials 2019, 31(38), 1800426., Reference 12, Teng et al., Mesoporous Organosilica Hollow Nanoparticles: Synthesis and Applications. Advanced Materials 2019, 31(38), 1707612.).At present, several hollow materials have been reported for phosphopeptide enrichment (Reference 13, Wu et al., Titania coated magnetic mesoporous hollow silica microspheres: fabrication and application to selective enrichment of phosphopeptides. Chemical Communications 2010, 46(47), 9031-9033., Reference 14, Lu et al., Facile synthesis of alumina hollow spheres for on-plate-selective enrichment of phosphopeptides. Chemical communications 2011, 47(18), 5334-6., Reference 15, Xu et al., Highly selective SiO2–NH2@TiO2 hollow microspheres for simultaneous enrichmentof phosphopeptides and glycopeptides. Analytical and Bioanalytical Chemistry 2017, 409(6), 1607-1614., Reference 16, Hong et al., Highly efficient enrichment of phosphopeptides from HeLa cells using hollow magnetic macro / mesoporous TiO2nanoparticles.Talanta 2018,187,223-230.), but their shells are either non-porous structures that do not have mass transfer capabilities and are unevenly coated, or the micron scale also involves the problems of slow mass transfer and high resistance encountered by the above-mentioned three-dimensional materials. Moreover, they are all materials developed based on MOAC. In other words, there are currently no hollow nanomaterials based on IMAC for phosphopeptide enrichment. Summary of the invention

[0004] The main content of the present invention includes a preparation of hollow nano-silicon spheres containing titanium ion functional groups based on a sol-gel reaction under neutral conditions and its application in phosphopeptide enrichment. First, a sol-gel reaction induced by potassium sulfate is used to prepare hollow nano-silicon spheres containing phosphonates, and the phosphonates in the hollow nano-silicon spheres are dealkylated to phosphoric acid groups after acidification with hydrochloric acid, and then chelated with titanium ions to finally obtain hollow nano-silicon spheres functionalized with titanium ions. Specifically, the following steps are included:

[0005] (1) Preparation of hollow nano-silica spheres containing phosphonate functional groups: 1.75-3.5 g potassium sulfate, 0.5-1 g F127, and 0.58-1.16 mL mesitylene are added to 30-60 mL water, and shaken at 13.5°C and 180-200 rpm for 12-14 hours. Then 1.19-2.38 mL tetramethoxysilane and 0.635-1.27 mL diethylphosphoethyltriethoxysilane are added, and the mixture is shaken for 24-26 hours, and then transferred to a hydrothermal reactor and heated at 100°C for 24-26 hours. The product is washed with water and ethanol for 3-6 times, respectively, and then extracted with ethanol Soxhlet for 24-26 hours and dried to obtain hollow nano-silica spheres containing phosphonate functional groups;

[0006] (2) Preparation of hollow nano-silica spheres functionalized with phosphoric acid: 0.2-0.35 g of the hollow nano-silica spheres containing phosphonate functional groups obtained in step (1) are added to 100-175 mL of concentrated hydrochloric acid, refluxed at 100-105° C. for 24-26 hours, then washed with water 3-6 times, washed with ethanol 1-2 times, and dried to obtain hollow nano-silica spheres functionalized with phosphoric acid.

[0007] (3) Preparation of hollow nano-silicon spheres functionalized with titanium ions: 30 to 60 mg of the hollow nano-silicon spheres functionalized with phosphoric acid obtained in step (2) are added to 15 to 30 mL of a titanium sulfate solution having a concentration of 100 to 200 mg / mL, and the mixture is shaken and reacted at room temperature for 12 to 14 hours. The mixture is washed with water, 0.1 to 0.5% trifluoroacetic acid, 100 to 200 mM sodium chloride / 0.1 to 0.5% trifluoroacetic acid, water, and ethanol in sequence, and then dried to finally obtain hollow nano-silicon spheres functionalized with titanium ions.

[0008] The obtained material can be used as a stationary phase for immobilized metal ion affinity chromatography for rapid, highly sensitive and highly selective enrichment of phosphopeptides. The characteristics of this method are that no acid or alkali needs to be added during the sol-gel reaction, the reaction conditions are mild, the requirements for reaction equipment are low, the subsequent functionalization steps are simple, and no additional deposition coating and sacrificial template steps are required to form a hollow structure. The obtained hollow nano-silicon sphere has a thin and uniform shell layer, and the pores on the shell layer are short and simple in structure, which is conducive to rapid mass transfer, and has low mass transfer resistance and higher site utilization.

[0009] The advantages of the method for preparing the titanium ion functionalized hollow nano silicon spheres are:

[0010] (1) No acid or alkali needs to be added during the sol-gel reaction, the reaction conditions are mild, and the requirements for reaction equipment are low;

[0011] (2) The subsequent functionalization steps are simple, and the required functional groups are directly introduced into the hollow nanosilicon spheres, without the need for additional deposition, coating, and sacrificial template steps to form the hollow structure;

[0012] The titanium ion functionalized hollow nano silicon sphere material has the advantages that:

[0013] (1) Uniform particle size, large specific surface area, thin shell, short pores on the shell and simple structure, which is conducive to rapid mass transfer, small mass transfer resistance and higher site utilization;

[0014] (2) It has good enrichment specificity and selectivity for phosphopeptides.

[0015] (3) The enrichment speed of phosphopeptides is fast, which greatly improves the enrichment efficiency.

[0016] (4) It is the first hollow material for phosphopeptide enrichment based on the IMAC method.

[0017] The present invention firstly uses diethylphosphoethyltriethoxysilane and tetramethoxysilane as silicon source monomers, F127 as a surfactant, mesitylene as a swelling agent, potassium sulfate as an auxiliary agent, and water as a solvent to prepare hollow nano-silicon spheres containing phosphonates by sol-gel reaction under neutral conditions, dealkylates the phosphonate groups in the hollow nano-silicon spheres into phosphate functional groups after acidification with hydrochloric acid, and then chelates titanium ions to obtain hollow nano-silicon spheres that can be used for phosphopeptide enrichment. The method firstly proposes using diethylphosphoethyltriethoxysilane and tetramethoxysilane as co-condensation monomers for sol-gel reaction, and the prepared phosphonate functionalized hollow nano-silicon spheres can be converted into hollow nano-silicon spheres modified with titanium ions by chemical reaction, and does not need to introduce functional groups by deposition and encapsulation, thereby avoiding problems such as uneven encapsulation and pore blockage, and does not need to form a hollow structure by sacrificial template, thereby simplifying the steps. In addition, the hollow nanospheres obtained by this method have a large specific surface area, a thin shell, short pores and a simple structure. They can enrich phosphopeptides quickly with good specificity and selectivity. They can be used for high-sensitivity and high-selectivity enrichment of phosphopeptides in biological samples. It is also the first hollow material for phosphopeptide enrichment based on the IMAC method. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Schematic diagram of the preparation process of hollow nanosilicon spheres containing titanium ion functional groups.

[0019] Figure 2Transmission electron microscopy images of (a) SHS-P_1; (b) SHS-Ti_1; (c) SHS-P_2; (d) SHS-Ti_2 and (e) SHS-P_3.

[0020] Figure 3 (a) Nitrogen adsorption-desorption isotherm and (b) pore size distribution of the material.

[0021] Figure 4 (a) Infrared spectrum of the material; (b) Enlarged infrared spectrum corresponding to the dotted box in (a) and (c) X-ray energy scattering spectrum of SHS-Ti_1.

[0022] Figure 5 MALDI-TOF MS spectra of β-casein hydrolysate. (a) Before enrichment, 500 fmol; after enrichment with SHS-Ti_1 (b) 500 fmol; (c) 100 fmol; (d) 5 fmol; (e) after enrichment with Ti3C2-5, 500 fmol. In the figure, (★) represents phosphopeptide; (☆) represents dephosphorylated peptide.

[0023] Figure 6 MALDI-TOF MS spectra of the mixture of BSA enzymatic hydrolysate and β-casein enzymatic hydrolysate. (a) Before enrichment, BSA: β-casein = 10:1; after enrichment with SHS-Ti_1 (b) BSA: β-casein = 10:1; (c) BSA: β-casein = 100:1; (d) BSA: β-casein = 1000:1. In the figure, (★) represents phosphopeptide; (☆) represents dephosphorylated peptide.

[0024] Figure 7 MALDI-TOF MS spectra of human serum samples (1uL). (a) Before enrichment; (b) After enrichment with SHS-Ti_1. In the figure, (★) represents phosphopeptides.

[0025] Table 1 Information of phosphopeptide samples detected in β-casein hydrolysate. In the table, ([pS]) represents the phosphorylation site; (S / N 1 ) represents the signal-to-noise ratio of phosphopeptides before enrichment; (S / N 2 ) represents the signal-to-noise ratio of phosphopeptides after enrichment with SHS-Ti_1. DETAILED DESCRIPTION

[0026] Example 1

[0027] Preparation of SHS-Ti_1 Hollow Nano-Silica Spheres and Their Application in Enrichment of Phosphopeptides from β-casein Hydrolyzed Samples

[0028] (1) 1.75 g potassium sulfate, 0.5 g F127 (EO106 PO 70 EO 106 , Sigma, product number P2443), and 0.58 mL of mesitylene were added to 30 mL of water and shaken at 13.5°C and 180 rpm for 12 hours. Then 1.19 mL of tetramethoxysilane and 0.635 mL of diethylphosphoethyltriethoxysilane were added, and the mixture was shaken for 24 hours before being transferred to a hydrothermal reactor and heated at 100°C for 24 hours. The product was washed with water and ethanol three times in sequence, then extracted with ethanol Soxhlet for 24 hours, and dried. The product was recorded as SHS-P_1.

[0029] (2) 0.2 g of the material obtained in step (1) was added to 100 mL of 36% concentrated hydrochloric acid, refluxed at 100° C. for 24 hours, then washed with water three times, washed with ethanol once, and dried. The product was recorded as SHS-PH.

[0030] (3) 60 mg of the material obtained in step (2) was added to 30 mL of 200 mg / mL titanium sulfate solution, and the mixture was shaken at room temperature for 12 h. The mixture was washed with water, 0.1% trifluoroacetic acid, 0.1% trifluoroacetic acid containing 200 mM sodium chloride, water, and ethanol in sequence, and then dried to obtain hollow nano-silicon spheres functionalized with titanium ions. The product was recorded as SHS-Ti_1.

[0031] Preparation of β-casein enzymatic digestion samples:

[0032] 0.5 mg of β-casein was dissolved in 2 mL of 100 mM ammonium bicarbonate solution (pH = 8.2), and 20 μg of trypsin was added. The solution was enzymolyzed in a 37°C water bath for 12 h to obtain a protease hydrolysis sample, which was packaged and freeze-dried and stored in a -20°C refrigerator for later use.

[0033] Preparation of bovine serum albumin enzymatic digestion samples:

[0034] Dissolve 2 mg of bovine serum albumin in 1 mL of 100 mM ammonium bicarbonate solution containing 8 M urea (pH = 8.2), add 80 μmol DL-1,4-dithiothreitol, keep constant temperature in a 37°C water bath for 2 hours, then add 40 μmol 2-iodoacetamide, react in the dark for 40 minutes, add 7 mL of 100 mM ammonium bicarbonate solution, then add 80 μg of trypsin, hydrolyze in a 37°C water bath for 18 hours, desalt, obtain protease hydrolyzed samples, package and freeze-dry, and store in a -20°C refrigerator for later use.

[0035] Enrichment of phosphopeptides:

[0036] 2 mg of SHS-Ti material was weighed into a centrifuge tube, and the material was balanced with 200 μL of loading solution (the volume ratio of acetonitrile, water, and trifluoroacetic acid was 50:47:3); then 200 μL of loading solution (containing 1 μg of β-casein hydrolysate) was added, and the mixture was shaken at 25°C and 1500 rpm for 1 min; then centrifuged for 2 min (25,000 g speed), and the supernatant was discarded; the mixture was washed three times with the loading solution to remove nonspecifically adsorbed peptides, each time for 1 min; then the phosphopeptides adsorbed on the material were eluted with 200 μL of 10% (mass percentage) ammonia water for 1 min, centrifuged, and the eluate was retained and analyzed using a matrix-assisted laser desorption / ionization-time of flight mass spectrometer (Matrix-Assisted Laser Desorption / Ionization-Time of Flight Mass Spectrometry, MALDI-TOF MS).

[0037] MALDI-TOF-MS mass spectrometry analysis:

[0038] 0.5 μL of sample was dropped on the MALDI target, and after it was naturally dried, 0.5 μL of 2,5-dihydroxybenzoic acid solution (25 mg / mL) was covered on the sample point as a matrix. After it was completely naturally dried, it was sent to the MALDI-TOF mass spectrometer for analysis.

[0039] Example 2

[0040] Preparation of SHS-Ti_2 hollow nano-silica spheres and their application in enrichment of phosphopeptides from β-casein hydrolyzed samples

[0041] (1) 3.5 g potassium sulfate, 1 g F127, and 1.16 mL mesitylene were added to 60 mL water and shaken at 13.5°C and 180 rpm for 12 hours. Then 2.38 mL tetramethoxysilane and 1.27 mL diethylphosphoethyltriethoxysilane were added and shaken for 24 hours. After that, the mixture was transferred to a hydrothermal reactor and heated at 100°C for 24 hours. The product was washed with water and ethanol three times respectively, then extracted with ethanol for 24 hours and dried. The product was recorded as SHS-P_2.

[0042] (2) 0.35 g of the material obtained in step (1) was added to 175 mL of 36% concentrated hydrochloric acid, refluxed at 100° C. for 24 hours, then washed with water three times, washed with ethanol once, and dried.

[0043] (3) 30 mg of the material obtained in step (2) was added to 15 mL of 200 mg / mL titanium sulfate solution, and the mixture was shaken at room temperature for 12 h. The mixture was washed with water, 0.1% trifluoroacetic acid, 0.1% trifluoroacetic acid containing 200 mM sodium chloride, water, and ethanol in sequence, and then dried to obtain hollow nano-silicon spheres functionalized with titanium ions. The product was recorded as SHS-Ti_2.

[0044] Example 3

[0045] The preparation of SHS-P_3 hollow nano silicon spheres is the same as in Example 1, except that:

[0046] During the preparation of phosphonate-functionalized hollow nano-silica spheres, the amount of tetramethoxysilane used in the reaction system was reduced to 0.74 mL, and the amount of diethylphosphoethyltriethoxysilane used was increased to 1.59 mL. The other preparation conditions and processes were the same as those of the phosphonate-functionalized hollow nano-silica spheres SHS-P_1 in Example 1, recorded as SHS-P_3.

[0047] Comparative Example 1

[0048] Ti3C2-5 material in published work to enrich phosphopeptides from β-casein enzymatic hydrolyzed samples

[0049] For comparison, the Ti3C2-5 material in the published work (Reference 17, L, et.al., Comparative evaluation of MAX-Ti3AlC2 and MXene-Ti3C2 as affinity chromatographic materials for highly selective enrichment of phosphopeptides. Nanoscale 2021, 13(5), 2923-2930.) was used to enrich the phosphopeptides in the β-casein enzymatic hydrolyzed sample under its optimized conditions. The enrichment process was as follows: 5 mg The Ti3C2-5 material was placed in a centrifuge tube and equilibrated with 400 μL of loading solution (the volume ratio of acetonitrile, trifluoroacetic acid, lactic acid and water was 70:5:8.3:16.7); then 200 μL of loading solution (containing 1 μg of β-casein hydrolysate) was added and the mixture was shaken at 25°C and 1500 rpm for 30 min; then centrifuged for 2 min (25,000 g speed) and the supernatant was discarded; the material was washed three times with the loading solution to remove nonspecific adsorbed peptides, each time for 10 min; then the material was washed once with 200 μL of elution solution 1 (the volume ratio of acetonitrile, trifluoroacetic acid and water was 30:0.5:69.5), and twice with 200 μL of elution solution 2 (the volume ratio of acetonitrile, trifluoroacetic acid and water was 80:0.5:19.5), each time for 10 min; then 200 μL The phosphopeptides adsorbed on the material were eluted with 10% (mass percentage) ammonia water for 30 min, centrifuged, and the eluate was retained. The subsequent analysis was the same as in Example 1.

[0050] Product characterization:

[0051] The morphology and structure of the material were characterized by transmission electron microscopy. Figure 2 As shown, it can be clearly observed that the phosphonate functionalized material SHS-P_1 ( Figure 2 a) and the phosphonate functionalized material SHS-P_2 (prepared in Example 2) Figure 2 c) all showed a typical hollow structure with a bright middle core region and a dark edge shell region, with a particle size of about 17 nm, a cavity diameter of about 10 nm, and a shell thickness of about 3.5 nm; after phosphonate dealkylation and titanium ion fixation, the titanium ion functionalized material SHS-Ti_1 ( Figure 2 b) and the titanium ion functionalized material SHS-Ti_2 (prepared in Example 2) Figure 2 d) all showed the same morphology as the phosphate functionalized material. The phosphonate functionalized material SHS-P_3 ( Figure 2e) A large number of non-hollow structure products appear, which indicates that the excessively high content of the phosphonate functional monomer diethylphosphoethyltriethoxysilane in the initial reaction system will lead to the formation of a large number of non-hollow structures.

[0052] The pore parameters of hollow nano-silicon spheres SHS-P_1 functionalized with phosphonate and hollow nano-silicon spheres SHS-Ti_1 functionalized with titanium ions were characterized by nitrogen adsorption-desorption isotherms. Figure 3 As shown in a, both SHS-P_1 and SHS-Ti_1 exhibit typical type I and type IV characteristics. Among them, the adsorption amount of the curve increases sharply at relatively low pressure, indicating the existence of micropores in the material, which originate from the shell layer in the hollow silicon sphere. The hysteresis loop of the curve in the relatively high pressure part indicates the existence of mesoporous hollow cavities, which is consistent with the results of transmission electron microscopy. The specific surface areas of SHS-P_1 and SHS-Ti_1 were calculated using the Brunauer-Emmett-Teller model, and the results were 495 and 396 m 2 / g. The total pore volume was calculated using the nitrogen adsorption at a relative pressure of 0.99, and the results were 0.90 cm 3 / g. According to the pore size distribution curve calculated by density functional theory (DFT), it can be seen that the pore size distribution of SHS-P_1 is mainly concentrated at 1.6 and 7.9nm, and the pore size distribution of SHS-Ti_1 is mainly concentrated at 1.6 and 7.6nm, which can also confirm the structure of shell micropores and cavity mesopores in the material.

[0053] Fourier transform infrared spectroscopy was used to characterize the functional groups of hollow nanosilica spheres SHS without phosphonate functionalization, phosphonate functionalized hollow nanosilica spheres SS-P before the removal of surfactant, phosphonate functionalized hollow nanosilica spheres SHS-P_1, phosphate functionalized hollow nanosilica spheres SHS-PH, and titanium ion functionalized hollow nanosilica spheres SHS-Ti_1. Figure 4 As shown in a and b, the five materials all showed the peaks at 3400, 1637, 1070, 792, 460 and 960 cm -1 The peaks on the left and right are respectively attributed to the stretching vibration and bending vibration of the hydroxyl groups in the surface adsorbed water, the asymmetric stretching vibration, symmetric stretching vibration, bending vibration of Si-O-Si and the vibration of Si-OH. Compared with SHS-P_1, a peak at 1349cm appeared in SS-P. -1 The peak at 1480 and 1395 cm-1 in SHS-P_1 corresponds to the stretching vibration of COC in surfactant F127, indicating that the surfactant was completely removed by ethanol Soxhlet extraction. -1The peaks correspond to the deformation vibration of the methyl group in the phosphonate group; located at 2986 and 2915 cm -1 The peaks at 2936, 1447 and 1371 cm-1 correspond to the asymmetric stretching vibration and symmetric stretching vibration of CH in the methyl group of the phosphonate group, respectively. -1 The peaks correspond to the vibration of -CH2 in the ethoxy group of the phosphonate group; located at 1414 and 674 cm -1 The peak corresponds to the vibration of -CH2 in Si–CH2 of the phosphonate group. These all confirm that a hydrolysis-condensation reaction occurred between tetramethoxysilane and diethylphosphoethyltriethoxysilane, and the phosphonate group was successfully modified. Compared with SHS-P_1, the infrared spectrum of SHS-PH has a peak at 2330cm -1 The broad peaks corresponding to the vibration of P-OH indicate that the phosphonoethyl group [-PO(OC2H5)2] in the phosphonate group is converted into the phosphate group [-PO(OH)2] through the dealkylation process. The ethoxyl group is at 2986, 2936, 2915, 1480, 1447, 1395 and 1371 cm -1 The peak at 2330 cm-1 disappeared completely in the infrared spectrum of SHS-PH, which also proved the success of the dealkylation process. -1 The broad peak in the infrared spectrum of SHS-Ti_1 is significantly weakened due to the chelation of P-OH and titanium ions, which confirms the successful fixation of titanium ions. In addition, the elemental characterization of the titanium ion functionalized hollow nano-silicon spheres SHS-Ti_1 was carried out by energy dispersive X-ray spectroscopy. Figure 4 As shown in (c), peaks corresponding to carbon, oxygen, silicon, phosphorus and titanium elements appeared in the energy scattering X-ray spectrum of SHS-Ti_1, indicating that the phosphonate functional groups and titanium ions were successfully introduced.

[0054] The titanium ion-modified hollow nano-silica spheres SHS-Ti_1 prepared in Example 1 were used as the stationary phase material for immobilized metal ion affinity chromatography to separate and enrich the phosphopeptides in the β-casein hydrolyzed sample, the mixed sample of β-casein hydrolyzate and bovine serum albumin hydrolyzate, and the 1uL human serum sample. The MALDI-TOF MS comparison before and after enrichment is shown in Figure 2. Figure 5 , Figure 6 and Figure 7 As shown in Figure 2. For 500 fmol of β-casein enzymatic hydrolyzed sample, before enrichment, there were a large number of high-abundance non-phosphopeptide signal peaks in the spectrum, and the signal of the phosphopeptide was strongly suppressed ( Figure 5 a); After enrichment, almost all non-phosphopeptides were removed, and three phosphopeptides were detected with significantly enhanced signals ( Figure 5b, Table 1), indicating that the material has a high specificity for phosphopeptide enrichment. In order to investigate the enrichment sensitivity of the material, 100fmol and 5fmol β-casein hydrolyzed samples were enriched respectively. For the 100fmol β-casein hydrolyzed sample, three phosphopeptides could still be detected after enrichment ( Figure 5 c). For 5 fmol β-casein enzymatic digestion sample ( Figure 5 d), a phosphopeptide can be detected after enrichment, indicating that the enrichment detection limit of this material is 5fmol, which has good enrichment sensitivity.

[0055] In order to investigate the selectivity of the material for phosphopeptide enrichment, bovine serum albumin hydrolysate was added to β-casein hydrolysate to simulate the complexity of actual biological samples. Figure 6 As can be seen in a, before enrichment, a large number of non-phosphopeptide signals occupied the mass spectrometry spectrum, while after SHS-Ti_1 enrichment ( Figure 6 b), the three phosphopeptides can be clearly detected, and the background is very clean. When the mixing ratio is increased to 100:1 ( Figure 6 c), we can still clearly detect the three target phosphopeptides with almost no interference from non-phosphopeptides. When the mixing ratio is further increased to 1000:1 ( Figure 6 d), the three target phosphopeptides can also be detected, but there is nonspecific adsorption interference from a small number of non-phosphopeptides, indicating that the enrichment selectivity of SHS-Ti_1 for phosphopeptides can reach 1000:1, which has a very high enrichment selectivity.

[0056] In order to investigate the feasibility of hollow nano-silica spheres SHS-Ti_1 for enriching phosphopeptides in actual biological samples, we applied it to enrich endogenous phosphopeptides in 1uL human serum samples. Figure 7 a), no phosphopeptides were detected. After SHS-Ti_1 enrichment ( Figure 7 b), all four target phosphopeptides were detected, and there was no interference from non-phosphopeptides, indicating that SHS-Ti_1 has good applicability to actual biological samples. It is worth mentioning that in most of the reported work involving phosphopeptide enrichment materials, the loading time of phosphopeptides exceeds 15 minutes and the elution time exceeds 10 minutes, while the loading time and elution time of this material in the phosphopeptide enrichment process are only 1 minute, indicating that this material is faster and more efficient in enriching phosphopeptides, which is conducive to the detection of unstable phosphopeptides in samples and greatly saves time costs, especially for the processing of large batches of samples.

[0057] For comparison, the Ti3C2-5 material in the published work was used to enrich the phosphopeptides in 500 fmol β-casein enzymatic hydrolyzed samples under optimized conditions. Figure 5 As shown in Figure e, although all three phosphopeptides were detected and the signals were greatly enhanced compared to before enrichment, there were many non-phosphopeptide interferences, and the enrichment specificity was not as good as that of hollow nanosilica spheres SHS-Ti_1.

[0058] Table 1

[0059]

[0060] The hollow nano-silica spheres containing phosphonate groups prepared by the sol-gel reaction under neutral conditions can be subjected to hydrochloric acid dealkylation and titanium ion chelation to obtain Ti for phosphopeptide enrichment. 4+ -IMAC hollow nano-silica spheres. The hollow nano-silica spheres have the advantages of rapid, efficient, good specificity, high selectivity and sensitivity in the enrichment of phosphopeptides. Among them, the fast enrichment speed and short time consumption are characteristics that most phosphopeptide enrichment materials do not have. The entire preparation process does not require deposition, coating and sacrificial template processes, and the shell layer is uniform and suitable for large-scale preparation.

Claims

1. A method for preparing hollow nano silicon spheres containing titanium ion functional groups, characterized in that: Using diethylphosphoethyltriethoxysilane and tetramethoxysilane as silicon source monomers, F127 (EO 106 PO 70 EO 106 ) as a surfactant, mesitylene as a swelling agent, potassium sulfate as an auxiliary agent, and water as a solvent, and a sol-gel reaction is used to prepare hollow nano-silicon spheres containing phosphonate; the phosphonate groups in the hollow nano-silicon spheres can be dealkylated to become phosphoric acid functional groups, and then chelate with titanium ions to obtain hollow nano-silicon spheres containing titanium ion functional groups; You can follow the steps below: (1) Preparation of hollow nano-silica spheres containing phosphonate functional groups: 1.75-3.5 g potassium sulfate, 0.5-1 g F127, and 0.58-1.16 mL mesitylene were added to 30-60 mL water, and the mixture was shaken at 13-14°C and 180-200 rpm for 12-14 hours; 1.19-2.38 mL tetramethoxysilane and 0.635-1.27 mL diethylphosphoethyltriethoxysilane were then added, and the mixture was shaken for 24-26 hours, and then transferred to a hydrothermal reactor and heated at 100-105°C for 24-26 hours; the product was washed with water and ethanol for 3-6 times, respectively, and then extracted with ethanol for 24-26 hours and dried to obtain hollow nano-silica spheres containing phosphonate functional groups; (2) Preparation of hollow nano-silica spheres functionalized with phosphoric acid: 0.2-0.35 g of the hollow nano-silica spheres containing phosphonate functional groups obtained in step (1) are added to 100-175 mL of concentrated hydrochloric acid having a mass concentration of 36-38%, refluxed at 100-105° C. for 24-26 hours, then washed with water 3-6 times, washed with ethanol 1-2 times, and dried to obtain hollow nano-silica spheres functionalized with phosphoric acid; (3) Preparation of hollow nano-silica spheres functionalized with titanium ions: 30-60 mg of the hollow nano-silica spheres functionalized with phosphoric acid obtained in step (2) were added to 15-30 mL of a 100-200 mg / mL titanium sulfate solution, and the mixture was reacted at room temperature for 12-14 h. The mixture was washed with water, a 0.1-0.5% trifluoroacetic acid aqueous solution, a 0.1-0.5% trifluoroacetic acid aqueous solution containing 100-200 mM sodium chloride, water, and ethanol in sequence, and then dried to obtain hollow nano-silica spheres functionalized with titanium ions.

2. The titanium ion functionalized hollow nano-silicon sphere prepared by the preparation method according to claim 1.

3. An application of the titanium ion functionalized hollow nano silicon spheres according to claim 2, characterized in that: The titanium ion functionalized hollow nano-silica sphere is used as an immobilized metal ion affinity chromatography stationary phase material to separate and enrich phosphopeptides in biological samples.

4. The use according to claim 3, characterized in that: The biological sample is one or more of human or animal body fluids, tissues or cell enzymatic hydrolysis samples.