A CH4-SCR denitration catalyst and preparation method thereof

By designing the catalyst structure of hollow H-Pd microsphere core, zirconium-tungsten composite oxide intermediate layer and alumina shell, the stability of the existing CH4-SCR catalyst in a water-sulfur poisoning environment is solved, and efficient NOx decomposition is achieved It is suitable for SCR denitrification of gas exhaust gas.

CN116251591BActive Publication Date: 2024-11-22NANJING HUANFU NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211725299.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-30
Publication Date
2024-11-22
Estimated Expiration
2042-12-30

AI Technical Summary

Technical Problem

The existing CH4-SCR denitrification catalysts have poor stability in water-sulfur poisoning environments, are difficult to widely use in industries, and methane activation is difficult, resulting in insufficient denitrification efficiency and stability.

Method used

The catalyst structure of the shell was prepared by hydrothermal and ultrasonic methods to optimize the molar ratio of Zr and W elements and the molar ratio of Zr and W elements and The mass ratio of H-Pd and Al2O3 forms a core-shell microreactor structure to improve the activity of the catalyst and resist water sulfur poisoning.

Benefits of technology

It achieves a NOx removal efficiency of more than 90% in the range of 450-630℃, a CH4 conversion rate of up to 99.73%, and has excellent anti-water sulfur poisoning performance, which is suitable for gas exhaust CH4-SCR denitrification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116251591B_ABST
    Figure CN116251591B_ABST
Patent Text Reader

Abstract

The present invention discloses a CH4-SCR denitration catalyst and a preparation method thereof. The microscopic particle structure of the catalyst is based on hollow Pd (H-Pd) microspheres as the core and zirconium-tungsten composite oxide (ZrWO) with strong surface acidity and excellent thermal stability. x ) as the middle layer and alumina (Al2O3) as the shell. H‑Pd microspheres were prepared by hydrothermal method, and ZrWO x , Al2O3 to wrap the catalyst, thereby forming a core-shell structure with three parts: core, middle layer and shell. The components of the catalyst of the present invention are environmentally friendly, have a wide active temperature window, excellent denitrification activity, and excellent stability against water-sulfur poisoning, and have good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention provides a CH4-SCR denitration catalyst and a preparation method thereof, which belongs to the field of environmentally friendly catalytic materials and air pollution control, and is particularly suitable for CH4-SCR denitration of fuel gas tail gas. Background Art

[0002] Nitrogen oxides (NO x ) is the main cause of haze and deterioration of atmospheric environmental quality. x The annual emission exceeds 16 million tons, making it the world's largest emitter. Among the existing flue gas denitrification technologies, ammonia selective catalytic reduction (NH3-SCR) NO x High efficiency and good stability have become the mainstream technology and development direction of flue gas denitrification at home and abroad. Although ammonia as a reducing agent has high denitrification efficiency and good N2 selectivity, it will corrode equipment, cause ammonia escape and generate secondary pollution, and it is easy to SO at low temperature. x The resulting NH4HSO4 deposit deactivates the denitrification catalyst. Therefore, the development of new reducing agents to replace ammonia has been a research hotspot and a major need in the field of SCR denitrification both domestically and internationally. Given its abundant reserves, widespread distribution, low cost, and availability, as well as the presence of CH4 in most exhaust gases, CH4 is considered the most promising reducing agent to replace NH3. CH4 is the most stable hydrocarbon molecule, making it very difficult to activate and prone to preferential oxidation with O2 in an oxygen-containing atmosphere. Therefore, the core of CH4-SCR denitrification technology lies in the selection of a suitable catalyst. Most technologies for CH4-SCR catalysts, both domestically and internationally, use molecular sieves such as H-Beta (CN201610268637.8, CN201711319123.1, CN201611270121.3, CN202111144477.3) and SSZ-13 (CN201711315106.0) as catalysts. However, these molecular sieves have poor water-sulfur stability, hindering widespread industrial application. Therefore, the development of catalysts with superior CH4-SCR performance and strong stability is a significant need in this field. Summary of the Invention

[0003] The purpose of the present invention is to provide a method for preparing a CH4-SCR denitrification catalyst with high activity and good resistance to water-sulfur poisoning in order to address the current status and problems of existing CH4-SCR denitrification catalysts.

[0004] The specific technical solutions of the present invention are:

[0005] A CH4-SCR denitrification catalyst, which uses hollow H-Pd microspheres as cores and zirconium-tungsten composite oxide (ZrWO x ) as the middle layer and aluminum oxide (Al2O3) as the shell;

[0006] Among them, the molar ratio of Zr and W elements is 1: (0.01~0.5), H-Pd:ZrWO x The mass ratio is 1: (1 to 15), Al2O3: H-Pd@ZrWO x The mass ratio is 1:(0.01~0.5);

[0007] The zirconium-tungsten composite oxide ZrWO x It is a metal composite oxide composed of zirconium oxide and tungsten oxide.

[0008] In some preferred technical solutions: the molar ratio of Zr and W elements is 1: (0.08-0.13), H-Pd: ZrWO x The mass ratio is 1: (5-10), Al2O3: H-Pd@ZrWO x The mass ratio is 1:(0.05~0.15).

[0009] A method for preparing the above-mentioned CH4-SCR denitration catalyst, the preparation steps of the catalyst are as follows:

[0010] (1) Preparation of H-Pd microspheres

[0011] Palladium salt, urea, distilled water and anhydrous ethanol are mixed to form a transparent solution A; solution A is transferred to an autoclave lined with polytetrafluoroethylene for a hydrothermal reaction; the reaction product is washed with anhydrous ethanol, vacuum dried and calcined to obtain H-Pd microsphere powder;

[0012] Wherein: the mass ratio of palladium salt to urea is (0.01-0.05):(0.01-0.02);

[0013] (2)H-Pd@ZrWO x Preparation

[0014] H-Pd, PVP and distilled water were mixed and stirred for 6 to 8 hours to obtain suspension B, and suspension B was filtered to obtain H-Pd functionalized particles;

[0015] Wherein: the mass ratio of PVP to H-Pd is (0.02-0.08): (0.01-0.04);

[0016] The H-Pd functionalized particles were ultrasonically dispersed in anhydrous ethanol to form a suspension C, and then tungsten salt and zirconium salt were weighed and added to the suspension C. After ultrasonic dispersion for 0.5 to 1 hour, a suspension D was formed. Ammonia solution was added dropwise to the suspension D until the pH reached 8 to 11. The suspension was then stirred at 60 to 80 ° C for 1 to 2 hours. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried, and calcined to obtain H-Pd@ZrWO x Powder.

[0017] (3)H-Pd@ZrWO x Preparation of @Al2O3

[0018] Will H-Pd@ZrWO x , PVP and distilled water were mixed and ultrasonically stirred for 6 to 8 hours to obtain suspension E. Suspension E was filtered to obtain H-Pd@ZrWO x Functionalized particles.

[0019] H-Pd@ZrWO x Functionalized particles were ultrasonically dispersed in anhydrous ethanol to form a suspension F. Aluminum salt was added to suspension F and ultrasonically dispersed for 0.5 to 1 hour to form a suspension H. Ammonia solution was added dropwise to suspension D until the pH reached 10 to 12. The suspension was then stirred at 70°C for 1 to 2 hours. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried, and calcined to obtain H-Pd@ZrWO. x @Al2O3 powder.

[0020] Among them, PVP and H-Pd@ZrWO x The mass ratio is (0.02~0.08):(0.01~0.04).

[0021] In the technical solution of the present invention: the palladium salt in step (1) is palladium nitrate; the hydrothermal reaction temperature is 160-210° C., and the hydrothermal time is 5-10 hours; the drying temperature is 60-80° C., and the drying time is 6-12 hours; the calcination temperature is 600-700° C., and the calcination time is 2-4 hours.

[0022] In the technical solution of the present invention: the zirconium salt in step (2) is zirconium chloride or zirconium nitrate, and the tungsten salt is ammonium paratungstate or ammonium metatungstate;

[0023] The drying temperature is 60-80° C., and the drying time is 6-12 hours; the calcination temperature is 600-700° C., and the calcination time is 2-4 hours.

[0024] In the technical solution of the present invention: the aluminum salt described in step (3) is aluminum acetate or aluminum nitrate; the drying temperature is 60-80°C, and the drying time is 6-12 hours; the calcination temperature is 600-700°C, and the calcination time is 2-4 hours.

[0025] In the technical solution of the present invention: the catalyst is used in CH4-SCR denitrification of exhaust gas.

[0026] Beneficial effects:

[0027] The catalyst of the present invention is suitable for CH4-SCR denitrification. The efficiency of CH4-SCR denitrification is greater than 90% within 450-630℃, the CH4 conversion rate is greater than 90% above 450℃, and the denitrification efficiency is as high as 99.73% at 480℃. It has strong resistance to water and sulfur poisoning. The microscopic particle structure of the catalyst adopts the design of core-shell microreactor. The hollow Pd structure can more effectively exert its CH4-SCR performance. ZrWO x The solid superacid coating provides rich acidic conditions for Pd, further enhancing CH4-SCR denitrification activity and N2 selectivity. The Al2O3 coating effectively resists the interference of water and sulfur on the catalyst and improves its thermal stability. Compared with existing CH4-SCR denitrification catalysts, the catalyst of this invention features environmentally friendly components, a wide active temperature window, excellent denitrification activity, and excellent resistance to water and sulfur poisoning, making it particularly suitable for CH4-SCR denitrification of exhaust gas. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 H-Pd@ZrWO was prepared for Examples 1-4. x @CH4-SCR denitrification efficiency diagram of Al2O3 catalyst. DETAILED DESCRIPTION

[0029] The present invention will be further described below with reference to the embodiments, but the protection scope of the present invention is not limited thereto.

[0030] The denitration performance evaluation method of the catalyst of the present invention is as follows: a simulated exhaust gas composition is used, wherein the inlet NO concentration is 1000ppm, the inlet CH4 concentration is 3000ppm, the O2 content is 5%, the inlet SO2 concentration is 200ppm, the H2O content is 10vol.%, and N2 is used as the carrier gas at a total gas flow rate of 1000mL / min. A CH4-SCR denitration reaction is carried out in a fixed-bed reaction system. 3mL of a catalyst with a particle size of 40-60 mesh is measured and loaded into a quartz tube reactor with an inner diameter of 10mm. The reaction space velocity (GHSV) is set to 20000h -1 , set the reaction temperature range to 350-700℃, and use flue gas analyzer to monitor NO online before and after the reaction. x and CH4 concentration changes.

[0031] Example 1:

[0032] (1) Preparation of H-Pd microspheres

[0033] 3g of palladium nitrate, 1g of urea, 100g of distilled water, and 30g of anhydrous ethanol were weighed in a container with a mass ratio of distilled water / anhydrous ethanol / palladium salt / urea of ​​1:0.3:0.03:0.01 and stirred vigorously for 1 hour to form a transparent solution A. Solution A was transferred to a polytetrafluoroethylene-lined autoclave and hydrothermally reacted at 160°C for 5 hours. The reaction product was washed with anhydrous ethanol, vacuum-dried at 60°C for 6 hours, and calcined at 600°C for 2 hours to obtain H-Pd microsphere powder.

[0034] (2)H-Pd@ZrWO x Preparation

[0035] According to the mass ratio of distilled water / PVP / H-Pd of 1:0.02:0.01, 0.5 g H-Pd, 1 g PVP and 50 g distilled water were weighed and placed in the same container and ultrasonically stirred for 6 h to obtain suspension B. After filtering suspension B, H-Pd functionalized particles were obtained.

[0036] According to the molar ratio of Zr and W elements of 1:0.08, H-Pd:ZrWO x The mass ratio of zirconium chloride to H-Pd was 1:5, and the mass ratio of anhydrous ethanol to H-Pd was 1:0.005. The functionalized particles obtained above were ultrasonically dispersed in 100 g of anhydrous ethanol to form a suspension C. Then, 4.109 g of zirconium chloride and 0.368 g of ammonium paratungstate were weighed and added to the suspension C. After ultrasonic dispersion for 0.5 h, a suspension D was formed. A dilute ammonia solution (NH3·H2O) was added dropwise to the suspension D until the pH reached about 10. The suspension was then reacted at 70°C with continuous stirring for 1 h. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried at 60°C for 6 h, and calcined at 600°C for 2 h to obtain H-Pd@ZrWO. x Powder.

[0037] (3)H-Pd@ZrWO x @Al2O 3x Preparation

[0038] According to distilled water / PVP / H-Pd@ZrWO x The mass ratio of H-Pd@ZrWO is 1:0.02:0.01, and 0.5 g H-Pd@ZrWO is weighed. x , 1g PVP and 50g distilled water were placed in the same container and ultrasonically stirred for 6h to obtain suspension E. After filtering suspension E, H-Pd@ZrWO x Functionalized particles. According to Al2O3:H-Pd@ZrWO x The mass ratio of anhydrous ethanol:H-Pd@ZrWO is 1:0.05. xThe mass ratio of the functionalized particles was 1:0.005. The functionalized particles obtained above were ultrasonically dispersed in 100 g of anhydrous ethanol to form a suspension F. Then, 40.037 g of aluminum acetate was weighed and added to the suspension F. After ultrasonic dispersion for 0.5 h, a suspension H was formed. A dilute ammonia solution (NH3·H2O) was added dropwise to the suspension D until the pH reached about 10. The suspension was then stirred at 70°C for 1 h. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried at 60°C for 6 h, and calcined at 600°C for 2 h to obtain H-Pd@ZrWO. x @Al2O3 powder.

[0039] (4) Catalyst denitrification performance evaluation see Figure 1 .

[0040] Example 2:

[0041] (1) Preparation of H-Pd microspheres

[0042] The preparation of H-Pd microsphere powder is the same as that in Example 1.

[0043] (2)H-Pd@ZrWO x Preparation

[0044] The preparation of H-Pd functionalized particles was the same as in Example 1.

[0045] According to the molar ratio of Zr and W elements of 1:0.08, H-Pd:ZrWO x The mass ratio of zirconium nitrate and ammonium metatungstate was 1:5, and the mass ratio of anhydrous ethanol to H-Pd was 1:0.005. The functionalized particles obtained above were ultrasonically dispersed in 100 g of anhydrous ethanol to form a suspension C. Then, 5.983 g of zirconium nitrate and 0.350 g of ammonium metatungstate were weighed and added to the suspension C. After ultrasonic dispersion for 0.5 h, a suspension D was formed. A dilute ammonia solution (NH3·H2O) was added dropwise to the suspension D until the pH reached about 10. The suspension was then reacted at 70°C with continuous stirring for 1 h. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried at 60°C for 6 h, and calcined at 600°C for 2 h to obtain H-Pd@ZrWO. x Powder.

[0046] (3)H-Pd@ZrWO x Preparation of @Al2O3

[0047] According to distilled water / PVP / H-Pd@ZrWO x The mass ratio of H-Pd@ZrWO is 1:0.02:0.01, and 0.5 g H-Pd@ZrWO is weighed. x , 1g PVP and 50g distilled water were placed in the same container and ultrasonically stirred for 6h to obtain suspension E. After filtering suspension E, H-Pd@ZrWO xFunctionalized particles. According to Al2O3:H-Pd@ZrWO x The mass ratio of anhydrous ethanol:H-Pd@ZrWO is 1:0.05. x The mass ratio of the functionalized particles was 1:0.005. The functionalized particles obtained above were ultrasonically dispersed in 100 g of anhydrous ethanol to form a suspension F. Then, 41.780 g of aluminum nitrate was weighed and added to the suspension F. After ultrasonic dispersion for 0.5 h, a suspension H was formed. A dilute ammonia solution (NH3·H2O) was added dropwise to the suspension D until the pH reached about 10. The suspension was then stirred at 70°C for 1 h. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried at 60°C for 6 h, and calcined at 600°C for 2 h to obtain H-Pd@ZrWO. x @Al2O3 powder.

[0048] (4) Catalyst denitrification performance evaluation see Figure 1 .

[0049] Example 3:

[0050] (1) Preparation of H-Pd microspheres

[0051] 5g of palladium nitrate, 2g of urea, 100g of distilled water, and 40g of anhydrous ethanol were weighed in a container with a mass ratio of distilled water / anhydrous ethanol / palladium salt / urea of ​​1:0.4:0.05:0.02 and stirred vigorously for 1 hour to form a transparent solution A. Solution A was transferred to a polytetrafluoroethylene-lined autoclave and hydrothermally reacted at 160°C for 5 hours. The reaction product was washed with anhydrous ethanol, vacuum-dried at 60°C for 6 hours, and calcined at 600°C for 2 hours to obtain H-Pd microsphere powder.

[0052] (2)H-Pd@ZrWO x Preparation

[0053] According to the mass ratio of distilled water / PVP / H-Pd of 1:0.08:0.04, 1g H-Pd, 2g PVP and 25g distilled water were weighed and placed in the same container under ultrasonic stirring for 6h to obtain suspension B. After filtering suspension B, H-Pd functionalized particles were obtained. According to the molar ratio of Zr and W elements of 1:0.13, H-Pd:ZrWO xThe mass ratio of zirconium nitrate and ammonium metatungstate was 1:10, and the mass ratio of anhydrous ethanol to H-Pd was 1:0.01. The functionalized particles obtained above were ultrasonically dispersed in 100 g of anhydrous ethanol to form a suspension C. Then, 22.121 g of zirconium nitrate and 2.213 g of ammonium metatungstate were weighed and added to the suspension C. After ultrasonic dispersion for 0.5 h, a suspension D was formed. A dilute ammonia solution (NH3·H2O) was added dropwise to the suspension D until the pH reached about 10. The suspension was then reacted at 70°C with continuous stirring for 1 h. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried at 60°C for 6 h, and calcined at 600°C for 2 h to obtain H-Pd@ZrWO. x Powder.

[0054] (3)H-Pd@ZrWO x Preparation of @Al2O3

[0055] According to distilled water / PVP / H-Pd@ZrWO x The mass ratio of H-Pd@ZrWO is 1:0.08:0.04, and 1g H-Pd@ZrWO is weighed. x , 2g PVP and 25g distilled water were placed in the same container and ultrasonically stirred for 6h to obtain suspension E. After filtering suspension E, H-Pd@ZrWO x Functionalized particles. According to Al2O3:H-Pd@ZrWO x The mass ratio of anhydrous ethanol:H-Pd@ZrWO is 1:0.15. x The mass ratio of the functionalized particles was 1:0.01. The functionalized particles obtained above were ultrasonically dispersed in 100 g of anhydrous ethanol to form a suspension F. Then, 27.854 g of aluminum nitrate was weighed and added to the suspension F. After ultrasonic dispersion for 0.5 h, a suspension H was formed. A dilute ammonia solution (NH3·H2O) was added dropwise to the suspension D until the pH reached about 10. The suspension was then stirred at 70°C for 1 h. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried at 60°C for 6 h, and calcined at 600°C for 2 h to obtain H-Pd@ZrWO. x @Al2O3 powder.

[0056] (4) Catalyst denitrification performance evaluation see Figure 1 .

[0057] Example 4:

[0058] (1) Preparation of H-Pd microspheres

[0059] 5g of palladium nitrate, 2g of urea, 100g of distilled water, and 40g of anhydrous ethanol were weighed in a container with a mass ratio of distilled water / anhydrous ethanol / palladium salt / urea of ​​1:0.4:0.05:0.02, and stirred vigorously for 2 hours to form a transparent solution A. Solution A was transferred to a polytetrafluoroethylene-lined autoclave and hydrothermally reacted at 210°C for 10 hours. The reaction product was washed with anhydrous ethanol, vacuum-dried at 80°C for 12 hours, and calcined at 700°C for 4 hours to obtain H-Pd microsphere powder.

[0060] (2)H-Pd@ZrWO x Preparation

[0061] The preparation of H-Pd functionalized particles was the same as in Example 3.

[0062] According to the molar ratio of Zr and W elements of 1:0.13, H-Pd:ZrWO x The mass ratio of zirconium nitrate to H-Pd was 1:10, and the mass ratio of anhydrous ethanol to H-Pd was 1:0.01. The functionalized particles obtained above were ultrasonically dispersed in 100 g of anhydrous ethanol to form a suspension C. Then, 22.121 g of zirconium nitrate and 2.213 g of ammonium metatungstate were weighed and added to the suspension C. After ultrasonic dispersion for 1 hour, a suspension D was formed. A dilute ammonia solution (NH3·H2O) was added dropwise to the suspension D until the pH reached about 12. The suspension was then reacted at 70°C with continuous stirring for 2 hours. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried at 80°C for 12 hours, and calcined at 700°C for 4 hours to obtain H-Pd@ZrWO. x Powder.

[0063] (3)H-Pd@ZrWO x @Al2O 3x Preparation

[0064] According to distilled water / PVP / H-Pd@ZrWO x The mass ratio of H-Pd@ZrWO is 1:0.08:0.04, and 1g H-Pd@ZrWO is weighed. x , 2g PVP and 25g distilled water were placed in the same container and ultrasonically stirred for 8h to obtain suspension E. After filtering suspension E, H-Pd@ZrWO x Functionalized particles. According to Al2O3:H-Pd@ZrWO x The mass ratio of anhydrous ethanol:H-Pd@ZrWO is 1:0.15. xThe mass ratio of the functionalized particles was 1:0.01. The functionalized particles obtained above were ultrasonically dispersed in 100 g of anhydrous ethanol to form a suspension F. Then, 27.854 g of aluminum nitrate was weighed and added to the suspension F. After ultrasonic dispersion for 0.5 h, a suspension H was formed. A dilute ammonia solution (NH3·H2O) was added dropwise to the suspension D until the pH reached about 10. The suspension was then stirred at 70°C for 1 h. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried at 80°C for 12 h, and calcined at 700°C for 4 h to obtain H-Pd@ZrWO. x @Al2O3 powder.

[0065] (4) Catalyst denitrification performance evaluation see Figure 1 .

Claims

1. A CH4-SCR denitration catalyst, characterized in that: The catalyst uses hollow H-Pd microspheres as the core and zirconium-tungsten composite oxide ZrWO x as the middle layer, with aluminum oxide Al2O3 as the shell; Among them, the molar ratio of Zr and W elements is 1: (0.01~0.5), H-Pd:ZrWO x The mass ratio of Al2O3:H-Pd@ZrWO is 1:(1~15), x The mass ratio is 1:(0.01~0.5); The zirconium-tungsten composite oxide ZrWO x It is a metal composite oxide composed of zirconium oxide and tungsten oxide.

2. The CH4-SCR denitration catalyst according to claim 1, characterized in that: The molar ratio of Zr and W elements is 1:(0.08~0.13), H-Pd:ZrWO x The mass ratio of Al2O3:H-Pd@ZrWO is 1:(5~10), x The mass ratio is 1:(0.05~0.15).

3. A method for preparing the CH4-SCR denitration catalyst according to claim 1, characterized in that: The preparation steps of the catalyst are as follows: (1) Preparation of H-Pd microspheres The palladium salt, urea, distilled water and anhydrous ethanol are mixed to form a transparent solution A; the solution A is transferred to an autoclave equipped with a polytetrafluoroethylene liner to perform a hydrothermal reaction, and the product after the reaction is washed with anhydrous ethanol, vacuum dried, and calcined to obtain H-Pd microsphere powder; Wherein: the mass ratio of palladium salt to urea is (0.01-0.05):(0.01-0.02); the hydrothermal reaction temperature is 160-210° C., and the hydrothermal time is 5-10 h; (2) H-Pd@ZrWO x Preparation H-Pd, PVP and distilled water were mixed and stirred for 6-8 hours to obtain suspension B, and suspension B was filtered to obtain H-Pd functionalized particles; Wherein: the mass ratio of PVP and H-Pd is (0.02~0.08):(0.01~0.04); The H-Pd functionalized particles were ultrasonically dispersed in anhydrous ethanol to form a suspension C, and then tungsten salt and zirconium salt were weighed and added to the suspension C. After ultrasonic dispersion for 0.5-1h, a suspension D was formed. Ammonia solution was added dropwise to the suspension D until the pH reached 8-11, and then the suspension was reacted at 60-80°C for 1-2h under continuous stirring. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried, and calcined to obtain H-Pd@ZrWOx powder. (3) H-Pd@ZrWO x @Preparation of Al2O3 Will H-Pd@ZrWO x , PVP and distilled water were mixed and ultrasonically stirred for 6-8h to obtain suspension E. Suspension E was filtered to obtain H-Pd@ZrWO x Functionalized particles; H-Pd@ZrWO x Functionalized particles were ultrasonically dispersed in anhydrous ethanol to form suspension F, aluminum salt was added to suspension F, and suspension H was formed after ultrasonic dispersion for 0.5-1h. Ammonia solution was added dropwise to suspension D until the pH reached 10-12, and then the suspension was reacted at 70°C for 1-2h under continuous stirring. The obtained product was filtered, washed with anhydrous ethanol, vacuum dried, and calcined to obtain H-Pd@ZrWO x @Al2O3 powder; Among them, PVP and H-Pd@ZrWO x The mass ratio is (0.02~0.08):(0.01~0.04).

4. The preparation method according to claim 3, characterized in that: The palladium salt in step (1) is palladium nitrate; the drying temperature is 60-80°C, and the drying time is 6-12 hours; the calcination temperature is 600-700°C, and the calcination time is 2-4 hours.

5. The preparation method according to claim 3, characterized in that: The zirconium salt described in step (2) is zirconium chloride or zirconium nitrate, and the tungsten salt is ammonium paratungstate or ammonium metatungstate; The drying temperature is 60-80° C., and the drying time is 6-12 hours; the calcination temperature is 600-700° C., and the calcination time is 2-4 hours.

6. The preparation method according to claim 3, characterized in that: The aluminum salt described in step (3) is aluminum acetate or aluminum nitrate; the drying temperature is 60-80° C., and the drying time is 6-12 hours; the calcination temperature is 600-700° C., and the calcination time is 2-4 hours.

7. Use of the catalyst according to claim 1 in CH4-SCR denitrification of exhaust gas.