A cement-based permeable crystalline waterproof material and preparation method thereof
By using raw materials such as Portland cement, quartz sand, active components and calcium ion supplements in cement-based permeable crystalline waterproofing materials, difficult-to-dissociate complexes are formed and pores are filled, thereby solving the problem of freeze-thawing in the existing technology. and rust problems, improving the waterproof performance and durability of concrete, achieving deeper penetration depth and chloride ion resistance.
Patent Information
- Application Number
- CN202211482573.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-11-24
AI Technical Summary
While the existing cement-based permeable crystalline waterproofing materials improve the waterproofing effect, they also have problems with freezing and thawing and corrosion of steel bars, which affects the durability of concrete and the life of the building.
It uses raw materials such as Portland cement, quartz sand, active components, calcium ion supplements, ethyl silicate, isooctyltriethoxysilane and silica sol to promote crystal growth by forming difficult-to-dissociate complexes. , fill pores and cracks, combine with water-reducing agent to improve the compactness and waterproof performance of concrete, and increase the resistance to chloride ion penetration through the modification of silica groups.
It significantly improves the waterproofing ability and durability of concrete, enhances the flexural and compressive resistance, improves the workability and waterproofing effect of concrete, while avoiding chloride ion penetration and extending the life of the building.
Smart Images

Figure BDA0003962310770000051 
Figure BDA0003962310770000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof building materials, in particular to a cement-based permeable crystalline waterproof material and a preparation method thereof. Background Art
[0002] Cement-based permeable crystalline waterproof material, referred to as CCCW, is usually made of silicate cement or ordinary silicate cement, quartz sand, etc. as the main ingredients, mixed with active chemical substances. Due to its good anti-seepage and self-repairing properties, and can prevent steel corrosion, harmless to the human body, it is widely used in engineering projects such as subways, bridge decks, water conservancy projects, sewage treatment plants, etc., and has achieved remarkable waterproofing effects.
[0003] The Chinese invention patent with application number 2010101695495 discloses a cement-based penetrating crystalline waterproof material, in which calcium chloride is used as a coagulant and calcium ion supplementer for the penetrating crystalline waterproof material. Although calcium chloride can improve the early strength and antifreeze properties of the product to a certain extent, chloride ions can promote freeze-thaw of concrete and corrosion of steel bars, which will affect the durability of concrete and the life of buildings in the long run.
[0004] In view of the above-mentioned related technologies, the inventors believe that cement-based permeable crystalline waterproof materials must meet both the waterproof effect and the durability of concrete. Summary of the invention
[0005] In order to ensure the durability of concrete while satisfying the waterproof effect, the present application provides a cement-based permeable crystalline waterproof material and a preparation method thereof.
[0006] The present application provides a cement-based permeable crystalline waterproof material and a preparation method thereof. The following technical scheme is adopted: A cement-based permeable crystalline waterproof material comprises the following raw materials in parts by weight:
[0007] 40-65 parts of Portland cement;
[0008] 20-40 parts of quartz sand;
[0009] Active ingredient 7-12 parts;
[0010] Calcium ion supplement 1-9 servings;
[0011] Ethyl silicate 5-7 parts;
[0012] 3-6 parts of isooctyltriethoxysilane;
[0013] 5-10 parts of silica sol.
[0014] By adopting the above technical scheme, the active components can form difficult-to-dissociate complexes with calcium ions and calcium hydroxide, forming crystals to block pores and cracks, thereby improving the compactness of concrete and improving the waterproof ability of concrete. Calcium ion supplementers supplement calcium ions for concrete, causing a common ion effect in the concrete, promoting the growth process of crystals, and improving the waterproof ability of concrete.
[0015] Ethyl silicate, isooctyltriethoxysilane and silica sol are mixed for reaction. The siloxy groups of ethyl silicate and isooctyltriethoxysilane react with a large number of highly active hydroxyl groups on the surface of nano-silica in silica sol, so that the Si-OH on the surface of the particles is partially or completely replaced by alkyl groups, and the water-transporting silicon oxygen chains increase, thereby having the ability to resist chloride ion penetration. Ethyl silicate and calcium hydroxide generate calcium silicate, which fills the pores and cracks in the concrete and improves the waterproof performance and strength of the concrete.
[0016] Optionally, the raw materials also include 1-3 parts of a water reducing agent.
[0017] By adopting the above technical solution, the water reducer can also be used as an anionic surfactant. Its molecules contain hydrophilic and hydrophobic groups, which can reduce the surface tension and interfacial tension of water in concrete, thereby playing the role of dispersion, wetting and lubrication, and improving the workability of concrete.
[0018] Optionally, the water reducing agent is one or more of calcium lignin sulfonate, sodium lignin sulfonate, and magnesium lignin sulfonate.
[0019] By adopting the above technical solution, calcium lignin sulfonate, sodium lignin sulfonate and magnesium lignin sulfonate are common water reducers and can also be used as anionic surfactants. Their molecules contain hydrophilic and hydrophobic groups, which can reduce the surface tension and interfacial tension of water in concrete and improve the fluidity and workability of concrete.
[0020] Optionally, the particle size of the quartz sand is 0.5-3 mm.
[0021] By adopting the above technical solution, quartz sand plays a role as a skeleton, and the use of fine-grained quartz sand reduces the generation of pores in the waterproof material, improves the material's own strength and density, and inhibits the shrinkage of the material.
[0022] Optionally, the active components are sodium citrate, sodium silicate and sodium carbonate.
[0023] By adopting the above scheme, the silicate and carbonate of sodium silicate and sodium carbonate generate precipitates with calcium ions, and sodium citrate can catalyze the silicate and carbonate with calcium ions to generate more stable precipitates that are insoluble in water, fill the pores of concrete, compact the cracks, and improve the waterproof ability of concrete.
[0024] Optionally, the calcium ion supplement is calcium magnesium carbonate and calcium sulfate.
[0025] By adopting the above scheme, calcium magnesium carbonate and calcium sulfate supplement calcium ions for concrete, and a common ion effect occurs in the concrete. The supplemented calcium ions form water-insoluble precipitates with other components, thereby improving the waterproof ability of the concrete.
[0026] Optionally, the weight ratio of calcium magnesium carbonate to calcium sulfate is (2-3):1.
[0027] By adopting the above scheme, calcium magnesium carbonate can not only provide calcium ions, but also promote the reaction of carbonate substances with calcium ions to generate water-insoluble calcium carbonate. Calcium magnesium carbonate combines with calcium sulfate to supplement the calcium ions of concrete, increasing the amount of calcium magnesium sulfate and significantly improving the waterproofing effect.
[0028] In a second aspect, the present application provides a method for preparing a cement-based permeable crystalline waterproof material, using the following technical solution:
[0029] A method for preparing a cement-based permeable crystalline waterproof material comprises the following steps:
[0030] Step 1, ethyl silicate, isooctyltriethoxysilane and silica sol are mixed, and stirred at a constant temperature of 25-35° C. for 25-40 minutes to obtain a mixture;
[0031] Step 2: Mix silicate cement, quartz sand, active components, calcium ion supplement and water reducing agent in a mixer, and then add the mixture in step 1 and mix well to obtain a cement-based penetrating crystalline waterproof material.
[0032] By adopting the above scheme, under dry conditions, the cement-based material is in a dormant state. When tiny cracks or pores appear inside the cement-based material, the active components of the cement-based material dissolve in water when water infiltrates, and the active components react with cement hydration products to form crystals, which penetrate into the concrete along the cracks inside the concrete, fill the pores and cracks in the concrete, and make the concrete dense, thereby improving its flexural and compressive resistance.
[0033] In addition, the siloxy groups of ethyl silicate and isooctyltriethoxysilane react with the highly active hydroxyl groups on the surface of nano-silicon dioxide in silica sol, so that the Si-OH on the surface of the particles is partially or completely replaced by alkyl groups, increasing the water-transmitting silicon oxygen chain, having the ability to resist chloride ion penetration, and improving the durability of concrete. The use of water reducers improves the workability of concrete, and also allows the waterproof material to have a deeper penetration depth, thereby improving the waterproof effect of concrete.
[0034] In summary, this application has the following beneficial effects:
[0035] 1. Since the present application adopts active components of sodium citrate, sodium silicate and sodium carbonate, the active components can form a water-insoluble precipitate with calcium ions, plugging the pores and cracks of the concrete, thereby improving the compactness of the concrete and improving the waterproof ability of the concrete.
[0036] 2. Since the present application uses calcium magnesium carbonate and calcium sulfate, the calcium ion supplementer supplements calcium ions for the concrete, and a common ion effect occurs in the concrete, which promotes the growth process of the crystal and improves the waterproof ability of the concrete.
[0037] 3. In the present application, ethyl silicate, isooctyltriethoxysilane and silica sol are mixed and reacted. The siloxy groups of ethyl silicate and isooctyltriethoxysilane react with a large number of highly active hydroxyl groups on the surface of nano-silicon dioxide in the silica sol, so that the Si-OH on the surface of the colloid particles is partially or completely replaced by alkyl groups, the water-transporting silicon oxygen chains are increased, and the silicate has the property of resisting chloride ion penetration. Ethyl silicate reacts with calcium hydroxide to generate calcium silicate, which fills the pores and cracks in the concrete and improves the waterproof performance and strength of the concrete. DETAILED DESCRIPTION
[0038] The present application is further described in detail below in conjunction with embodiments and comparative examples.
[0039] The sources of raw materials for the following embodiments and comparative examples are provided: the raw materials for the embodiments and comparative examples can all be purchased commercially.
[0040] Embodiment of a method for preparing a cement-based permeable crystalline waterproof material
[0041] Example 1
[0042] A method for preparing a cement-based permeable crystalline waterproof material comprises the following steps:
[0043] Step 1, adding ethyl silicate, isooctyltriethoxysilane and silica sol into a blender, stirring at a constant temperature of 25-35° C. for 25-40 minutes to obtain a mixture;
[0044] Step 2: Stir silicate cement, quartz sand, sodium citrate, sodium silicate, sodium carbonate, calcium magnesium carbonate, calcium sulfate, calcium lignin sulfonate and magnesium lignin sulfonate in a mixer for 20 minutes, the weight ratio of sodium citrate, sodium silicate and sodium carbonate is 1:2:2, the particle size of quartz sand is 2 mm, the weight ratio of calcium magnesium carbonate and calcium sulfate is 2.5:1, the weight ratio of calcium lignin sulfonate and magnesium lignin sulfonate is 1:1, and then add the mixture in step 1 and stir for 15 minutes to obtain a cement-based penetrating crystalline waterproof material.
[0045] Example 2
[0046] A method for preparing a cement-based permeable crystalline waterproof material, which is different from Example 1 in that the water reducer is sodium lignin sulfonate, the particle size of quartz sand is 0.5 mm, and the weight ratio of magnesium calcium carbonate to calcium sulfate is 2:1.
[0047] Example 3
[0048] A method for preparing a cement-based permeable crystalline waterproof material, which is different from Example 1 in that the particle size of calcium lignin sulfonate and quartz sand is 3 mm, and the weight ratio of calcium magnesium carbonate and calcium sulfate is 3:1.
[0049] The components of the raw materials of Examples 1-3 and their corresponding weight fractions are shown in Table 1.
[0050] Table 1 Components and their mass (kg) in Examples 1-3
[0051] Components Example 1 Example 2 Example 3 Portland cement 50 40 65 Quartz sand 30 20 40 Sodium Citrate 2 1.4 2.4 Sodium silicate 4 2.8 4.8 Sodium carbonate 4 2.8 4.8 Calcium magnesium carbonate 5 0.68 6.75 Calcium sulfate 2 0.34 2.25 Ethyl silicate 6 7 5 Isooctyltriethoxysilane 4 3 6 Silica Sol 8 5 10 Calcium lignin sulfonate — — 3 Magnesium lignin sulfonate 1 — — Calcium lignin sulfonate 1 — — Sodium lignin sulfonate — 1 —
[0052] Example 4
[0053] A method for preparing a cement-based permeable crystalline waterproof material, which is different from Example 2 in that the particle size of the quartz sand is 0.2 mm.
[0054] Example 5
[0055] A method for preparing a cement-based permeable crystalline waterproof material, which is different from Example 3 in that the particle size of the quartz sand is 4 mm.
[0056] Example 6
[0057] A method for preparing a cement-based permeable crystalline waterproof material, which is different from Example 2 in that the amount of magnesium calcium carbonate is 0.51 kg, the amount of calcium sulfate is 0.51 kg, and the weight ratio of magnesium calcium carbonate to calcium sulfate is 1:1.
[0058] Example 7
[0059] A method for preparing a cement-based permeable crystalline waterproof material, which is different from Example 3 in that magnesium calcium carbonate is 3 kg, calcium sulfate is 6 kg, and the weight ratio of magnesium calcium carbonate to calcium sulfate is 1:2.
[0060] Comparative Example
[0061] Comparative Example 1
[0062] A method for preparing a cement-based permeable crystalline waterproof material, which is different from Example 1 in that the raw materials do not include ethyl silicate, isooctyltriethoxysilane and silica sol.
[0063] Comparative Example 2
[0064] A method for preparing a cement-based permeable crystalline waterproof material, which is different from Example 1 in that the active component does not include sodium citrate, and the calcium ion supplement does not include magnesium calcium carbonate.
[0065] Performance testing experimental samples: The cement-based penetrating crystalline waterproof materials prepared in Examples 1-7 and Comparative Examples 1-3 were used as experimental samples.
[0066] Experimental method: According to the method specified in the national standard GB18445-2012 (cement-based penetrating crystalline waterproof material), the 28d compressive strength (MPa), 28d impermeability pressure ratio (with coating) and 28d impermeability pressure ratio (without coating) performance of the waterproof material were tested.
[0067] Table 2 Performance test results
[0068]
[0069]
[0070] Combining Examples 2-3 and 4-5, and Table 2, it can be seen that the performance of Example 2-3 is better than that of Example 4-5, proving that the particle size of quartz sand is too fine, filling the pores of concrete, although it hinders other active components from entering the pores of concrete, reducing the waterproof effect, and large-particle quartz sand produces more pores, resulting in reduced strength and waterproof performance.
[0071] Combining Examples 2-3 and Examples 6-7, and combining with Table 2, it can be seen that the performance of Example 2-3 is better than that of Example 6-7. In the calcium ion supplement, magnesium calcium carbonate and magnesium calcium sulfate are added to provide calcium ions and promote the reaction of carbonate substances with calcium ions to generate water-insoluble calcium carbonate. Therefore, appropriately increasing the proportion of magnesium calcium carbonate can significantly improve the waterproof effect of concrete.
[0072] Combining Example 1 with Comparative Examples 1-2 and Table 2, it can be seen that the performance of Example 1 is better than that of Comparative Examples 1-2, which proves that the siloxy groups of ethyl silicate and isooctyltriethoxysilane react with a large number of highly active hydroxyl groups on the surface of nano-silicon dioxide in the silica sol, so that the Si-OH on the surface of the colloid particles is partially or completely replaced by alkyl, the water-transporting silicon oxygen chain increases, the resistance to chloride ion penetration is increased, and the waterproof performance of the concrete is improved. Ethyl silicate and calcium hydroxide generate calcium silicate, which fills the pores and cracks in the concrete and improves the waterproof performance and strength of the concrete.
[0073] Calcium magnesium carbonate combined with calcium sulfate can significantly improve the waterproof effect of concrete while supplementing calcium ions. Sodium citrate can catalyze silicate and carbonate to react with calcium ions to form a more stable precipitation that is insoluble in water, greatly improving the waterproof performance of concrete.
[0074] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A cement-based permeable crystalline waterproof material, characterized in that: It is composed of the following raw materials in parts by weight: 40-65 parts of Portland cement; 20-40 parts of quartz sand; Active ingredient 7-12 parts; Calcium ion supplement 1-9 servings; Ethyl silicate 5-7 parts; 3-6 parts of isooctyltriethoxysilane; Silica sol 5-10 parts; 1-3 parts of water reducing agent; The active components are sodium citrate, sodium silicate and sodium carbonate, added in a weight ratio of 1:2:2; the particle size of the quartz sand is 0.5-3 mm; the calcium ion supplement is calcium magnesium carbonate and calcium sulfate, added in a weight ratio of (2-3):1; The preparation comprises the following steps: Step 1, ethyl silicate, isooctyltriethoxysilane and silica sol are mixed, and stirred at a constant temperature of 25-35° C. for 25-40 minutes to obtain a mixture; Step 2: Mix silicate cement, quartz sand, active components, calcium ion supplement and water reducing agent in a mixer, and then add the mixture in step 1 and mix well to obtain a cement-based penetrating crystalline waterproof material.
2. The cement-based permeable crystalline waterproof material according to claim 1, characterized in that: The water reducing agent is one or more of calcium lignin sulfonate, sodium lignin sulfonate and magnesium lignin sulfonate.