Fluorine-containing allyl compound, modified bismaleimide resin, and preparation method and application thereof

By modifying bismaleimide resin with fluorinated allyl compounds, a highly cross-linked ladder structure is generated, which solves the shortcomings of resin substrates in terms of heat resistance, water absorption and dielectric properties, making it suitable for high-frequency and high-speed printed circuit boards.

CN116253625BActive Publication Date: 2024-11-26GUANGDONG HINNO TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211694316.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-11-26
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare resin substrates that possess excellent heat resistance, low water absorption, high modulus, and low dielectric constant and dielectric loss, especially bismaleimide resins, which limits their application in high-frequency and high-speed printed circuit boards.

Method used

A fluorinated allyl compound was used to modify bismaleimide resin, and a highly cross-linked ladder-structure modified bismaleimide resin was generated through ene addition reaction and Diels-Alder cyclization reaction. A resin composition was prepared by combining cyanate ester resin and functional resin.

Benefits of technology

The modified bismaleimide resin achieves heat resistance, low water absorption, and excellent dielectric properties, making it suitable for high-density interconnect integrated circuit packaging and high-frequency, high-speed printed circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116253625B_ABST
    Figure CN116253625B_ABST
Patent Text Reader

Abstract

The present invention relates to a fluorine-containing allyl compound, a modified bismaleimide resin, and a preparation method and application thereof. The fluorine-containing allyl compound has a structure shown in formula (I). When used in the modified bismaleimide resin, the modified bismaleimide resin can have the advantages of excellent heat resistance, low water absorption, high modulus, low dielectric constant and dielectric loss. The fluorine-containing allyl compound can be further used to prepare resin compositions, prepregs, laminates and printed circuit boards, and is applied to the fields of high-performance printed circuit boards such as high-density interconnect integrated circuit packaging, high-frequency and high-speed. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer modification, and in particular to a fluorine-containing allyl compound, a modified bismaleimide resin, and a preparation method and application thereof. Background Art

[0002] With the rapid development of the electronics industry, the components of electronic products are constantly developing in the direction of light, thin, short and small. Electronic components require higher signal propagation speed and transmission efficiency. As a result, the market demand for high-frequency and high-speed printed circuit boards is increasing. Therefore, higher requirements are also placed on the copper-clad laminate as a carrier and the resin substrate used.

[0003] At present, a scheme for preparing a high-frequency resin composition with excellent dielectric properties by compounding a fluorinated benzoxazine prepolymer with an epoxy resin has been reported. The fluorinated benzoxazine prepolymer has an oxazine ring structure, which can reduce the concentration of hydroxyl groups generated when the resin is cured, and relatively increase the content of benzene rings, greatly reducing the dielectric constant and dielectric loss of the product. However, due to the addition of a large amount of benzoxazine, it is easy to cause insufficient heat resistance and a decrease in high-temperature modulus.

[0004] Bismaleimide resin (BMI) has excellent heat resistance and thermal stability, low curing shrinkage, and good thermal expansion performance, making it a commonly used resin matrix in high-performance copper-clad laminates. However, unmodified bismaleimide has poor solubility, high cross-linking density, and brittle cured properties, making it difficult to use alone and must be modified by a modifier before use. In traditional technology, diamine-modified bismaleimide resins are often used to prepare substrates for electrical boards, but they have defects such as high curing temperature, high water absorption, and high dielectric constant and loss values.

[0005] In summary, how to obtain a new type of modifier and use it for bismaleimide resin modification to prepare a resin substrate with excellent heat resistance, low water absorption, high modulus, and low dielectric constant and dielectric loss value has always been a difficult problem in this field. Summary of the invention

[0006] Based on this, the present invention provides a new type of modifier, which is used for modifying bismaleimide resin to prepare modified bismaleimide resin with excellent heat resistance, low water absorption, high modulus, low dielectric constant and dielectric loss, which can be used to prepare resin compositions, prepregs, laminates and printed circuit boards.

[0007] The technical solution is as follows:

[0008] A fluorine-containing allyl compound having a structure shown in formula (I):

[0009]

[0010] The present invention also provides a method for preparing the fluorine-containing allyl compound as described above, comprising the following steps:

[0011] Mixing hexafluorobisphenol AF, a base and a catalyst in a solvent to prepare a suspension;

[0012] The suspension is mixed with allyl bromide and reacted.

[0013] In one embodiment, the molar ratio of hexafluorobisphenol AF, alkali and propylene bromide is 1:(0.2-4):(0.2-6).

[0014] In one embodiment, the base is selected from one or more of potassium carbonate, cesium carbonate, sodium carbonate, potassium hydroxide, sodium hydroxide, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide.

[0015] In one embodiment, the catalyst is selected from one or more of potassium iodide, cesium iodide and sodium iodide.

[0016] The present invention also provides a modified bismaleimide resin, the raw materials of which include a modifier and a bismaleimide resin;

[0017] The modifier includes a fluorine-containing allyl compound as shown in the above formula (I);

[0018]

[0019] In one of the embodiments, the mass ratio of the fluorine-containing allyl compound to the bismaleimide resin is (0.5-1):1.

[0020] In one embodiment, the modifier further comprises one or more of 2,2'-diallyl bisphenol A, 2,2'-diallyl bisphenol S, 2,2'-diallyl bisphenol F and bisphenol A bisallyl ether.

[0021] In one embodiment, the bismaleimide resin contains two or more maleimide groups.

[0022] In one embodiment, the monomer of the bismaleimide resin is selected from one or more of N-phenylmaleimide, N-(2-methylphenyl)maleimide, N-(4-methylphenyl)maleimide, N-(2,6-dimethylphenyl)maleimide, bis(4-maleimidophenyl)methane, 2,2-bis(4-(4-maleimidophenoxy)-phenyl)propane, bis(3,5-dimethyl-4-maleimidophenyl)methane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bis(3,5-diethyl-4-maleimidophenyl)methane, polyphenylmethane bismaleimide, bismaleimide containing biphenyl structure and polymaleimide.

[0023] The present invention also provides a method for preparing the modified bismaleimide resin as described above, comprising the following steps:

[0024] The modifier is mixed with bismaleimide resin and reacted at 100°C to 150°C.

[0025] In one embodiment, the reaction time is 60 min to 120 min.

[0026] In one embodiment, the method for preparing the modified bismaleimide resin further comprises the following step of preparing a fluorine-containing allyl compound represented by formula (I):

[0027] Mixing hexafluorobisphenol AF, a base and a catalyst in a solvent to prepare a suspension;

[0028] The suspension is mixed with allyl bromide and reacted.

[0029] The present invention also provides the application of the modified bismaleimide resin as described above, and the technical scheme is as follows:

[0030] A resin composition comprising the following components in parts by weight:

[0031] 30 to 80 parts of the modified bismaleimide resin as described above;

[0032] 20 to 60 parts of cyanate resin; and

[0033] 5 to 20 parts of functional resin.

[0034] In one embodiment, the cyanate ester resin is selected from one or more of bisphenol A cyanate ester resin, phenolic cyanate ester resin, bisphenol F cyanate ester resin, multifunctional cyanate ester resin, bisphenol M cyanate ester resin, bisphenol E cyanate ester resin and dicyclopentadiene bisphenol cyanate ester resin.

[0035] In one embodiment, the functional resin is selected from one or more of epoxy resin, benzoxazine and polybutadiene.

[0036] In one embodiment, the resin composition further comprises one or more of a flame retardant, a filler, a curing accelerator, a coupling agent and a toughening agent.

[0037] In one embodiment, the resin composition includes 5 to 20 parts of flame retardant and 0 to 40 parts of filler, by weight.

[0038] In one embodiment, the flame retardant is selected from one or more of decabromodiphenylethane, tetrabromobisphenol A, brominated epoxy resin, phosphorus-containing epoxy resin, phosphorus-containing phenolic resin, phosphazene compound, phosphate ester compound and phosphorus-containing cyanate ester.

[0039] In one embodiment, the filler is selected from one or more of zirconium vanadate, zirconium tungstate, hafnium tungstate, glass-ceramics, eucryptite, silicon dioxide, quartz, mica powder, titanium dioxide, magnesium oxide, magnesium hydroxide, talc, aluminum oxide, silicon carbide, boron nitride, aluminum nitride, molybdenum oxide, barium sulfate, zinc molybdate, zinc borate, zinc stannate, zinc oxide, strontium titanate, barium titanate, calcium titanate, clay and kaolin.

[0040] A prepreg comprises the modified bismaleimide resin as described above, or the resin composition as described above.

[0041] A laminated board comprises the modified bismaleimide resin as described above, or the resin composition as described above, or the prepreg as described above.

[0042] In one embodiment, the laminate further includes at least one layer of metal foil located on one side or both sides of the prepreg.

[0043] A printed circuit board comprises the modified bismaleimide resin as described above, or the resin composition as described above, or the prepreg as described above, or the laminate as described above.

[0044] The present invention has the following beneficial effects:

[0045] The present invention provides a fluorine-containing allyl compound shown in formula (I), and a modifier containing the fluorine-containing allyl compound shown in formula (I) is used to modify bismaleimide, wherein due to the electron-withdrawing effect of the carbonyl group in the molecular structure of the bismaleimide, the carbon-carbon unsaturated double bond is an electron-deficient double bond, the double bond and the fluorine-containing allyl compound first undergo an ene addition reaction to generate an intermediate, and the double bond of BMI undergoes a Diels-Alder ring-forming reaction with the intermediate to finally generate a ladder-structured modified bismaleimide resin with a high degree of crosslinking, which has excellent heat resistance, low water absorption, high modulus, and low dielectric constant and dielectric loss.

[0046] The modified bismaleimide resin is used to prepare a resin composition, which also has excellent heat resistance, low water absorption, high modulus and excellent dielectric properties. It can be used to prepare prepregs and laminates, and further applied to high-performance printed circuit board fields such as high-density interconnect integrated circuit packaging, high frequency and high speed. DETAILED DESCRIPTION

[0047] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0049] In the present invention, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are considered continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0050] The temperature parameters in the present invention, if not specifically limited, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument.

[0051] In the present invention, when it comes to the unit of the data range, if there is a unit only after the right endpoint, it means that the units of the left endpoint and the right endpoint are the same. For example, 150-160°C means that the units of the left endpoint "150" and the right endpoint "160" are both ℃ (Celsius).

[0052] In the present invention, in the description of the invention, the meaning of "several" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0053] If not otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution.

[0054] If not otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0055] Where “including,” “having,” and “comprising” are used herein, it is intended to cover a non-exclusive inclusion, and another component may also be added unless explicit limiting terms such as “only,” “consisting of,” etc. are used.

[0056] Unless mentioned to the contrary, terms in the singular may include plural forms and should not be construed as being one in number.

[0057] The invention provides a novel modifier, which is used for modifying bismaleimide resin to prepare modified bismaleimide resin with excellent heat resistance, low water absorption, high modulus, low dielectric constant and dielectric loss, and can be used to prepare resin compositions, prepregs, laminates and printed circuit boards.

[0058] The technical solution is as follows:

[0059] A fluorine-containing allyl compound having a structure shown in formula (I):

[0060]

[0061] The present invention also provides a method for preparing the fluorine-containing allyl compound as described above, comprising the following steps:

[0062] Mixing hexafluorobisphenol AF, a base and a catalyst in a solvent to prepare a suspension;

[0063] The suspension is mixed with allyl bromide and reacted.

[0064] In one embodiment, the molar ratio of hexafluorobisphenol AF to the base is 1:(0.2-4).

[0065] In one embodiment, the base is selected from one or more of potassium carbonate, cesium carbonate, sodium carbonate, potassium hydroxide, sodium hydroxide, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide.

[0066] In one of the embodiments, the mass ratio of hexafluorobisphenol AF to the catalyst is 100:(0.1-10).

[0067] In one embodiment, the catalyst is selected from one or more of potassium iodide, cesium iodide and sodium iodide.

[0068] In one embodiment, the molar ratio of hexafluorobisphenol AF to allyl bromide is 1:(0.2-6).

[0069] In one embodiment, the solvent is selected from one or more of acetone, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, methyltetrahydrofuran and dimethyl sulfoxide.

[0070] In one embodiment, the suspension is mixed with allyl bromide, and the reaction step is carried out in a protective gas atmosphere (such as nitrogen or argon).

[0071] In one embodiment, the preparation steps of the fluorine-containing allyl compound represented by formula (I) are as follows:

[0072] 1. Weigh hexafluorobisphenol AF (0.4 mol, 134.5 g) and place it in a three-necked bottle. Measure 300 mL of acetone and stir to completely dissolve it. Weigh anhydrous potassium carbonate (0.1 mol, 138.2 g) and potassium iodide (3 wt.% hexafluorobisphenol AF, 4.035 g) and place them in the bottle. Adjust the speed to suspend the solid in the solution.

[0073] 2. Add allyl bromide (0.1 mol, 120.98 g) in a nitrogen atmosphere, and stir and reflux under nitrogen atmosphere at 60°C for 26 hours. Finally, the reaction status was detected by spot plate;

[0074] 3. After the reaction is completed, remove the potassium carbonate and potassium iodide solids by suction filtration; remove the acetone from the liquid by vacuum distillation;

[0075] 4. The liquid obtained after reduced pressure distillation is purified by column chromatography (eluent: pure petroleum ether), and the petroleum ether is removed by rotary evaporation to obtain a colorless oily liquid, which is dried to obtain the fluorine-containing allyl compound represented by formula (I), named 2,2-bis(4-allyloxyphenyl)hexafluoropropane.

[0076] The present invention also provides a modified bismaleimide resin, the raw materials of which include a modifier and a bismaleimide resin;

[0077] The modifier includes a fluorine-containing allyl compound represented by formula (I);

[0078]

[0079] The present invention uses a modifier comprising a fluorine-containing allyl compound shown in formula (I) to modify bismaleimide, wherein due to the electron-withdrawing effect of the carbonyl group in the molecular structure of bismaleimide, the carbon-carbon unsaturated double bond is an electron-deficient double bond, the double bond and the fluorine-containing allyl compound first undergo an ene addition reaction to generate an intermediate, and the double bond of BMI undergoes a Diels-Alder ring-forming reaction with the intermediate to finally generate a ladder-structured modified bismaleimide resin with a high degree of crosslinking, which has excellent heat resistance, low water absorption, high modulus, and low dielectric constant and dielectric loss.

[0080] In one embodiment, the mass ratio of the fluorine-containing allyl compound to the bismaleimide resin is (0.5-1):1. If the fluorine-containing allyl compound is too little, the improvement effect on the electrical properties of the bismaleimide resin is limited, and too much fluorine-containing allyl compound will affect the processing performance of the bismaleimide resin. It can be understood that the mass ratio of the fluorine-containing allyl compound to the bismaleimide resin includes but is not limited to 0.5:1, 0.55:1, 0.6:1, 0.65:1, 0.7:1, 0.75:1, 0.8:1, 0.85:1, 0.9:1, 0.95:1 and 1:1. Preferably, the mass ratio of the fluorine-containing allyl compound to the bismaleimide resin is (0.5-0.8):1.

[0081] In one embodiment, the modifier further comprises one or more of 2,2'diallyl bisphenol A, 2,2'diallyl bisphenol S, 2,2'diallyl bisphenol F and bisphenol A bisallyl ether. The fluorinated allyl compound and these modifiers are used in combination to give the bismaleimide resin substrate better adhesion.

[0082] Preferably, in one embodiment, the modifier is prepared by compounding a fluorine-containing allyl compound represented by formula (I) and 2,2'-diallyl bisphenol A in a mass ratio of (0.1-10):1.

[0083] Preferably, in one embodiment, the modifier is prepared by compounding a fluorine-containing allyl compound represented by formula (I) and 2,2'-diallyl bisphenol S in a mass ratio of (0.1-10):1.

[0084] Preferably, in one of the embodiments, the modifier is prepared by compounding a fluorine-containing allyl compound represented by formula (I) and diallyl bisphenol F in a mass ratio of (0.1-10):1.

[0085] Preferably, in one of the embodiments, the modifier is prepared by compounding a fluorine-containing allyl compound represented by formula (I) and bisphenol A bisallyl ether in a mass ratio of (0.1-10):1.

[0086] In one embodiment, the bismaleimide resin contains two or more maleimide groups.

[0087] In one embodiment, the monomer of the bismaleimide resin is selected from one or more of N-phenylmaleimide, N-(2-methylphenyl)maleimide, N-(4-methylphenyl)maleimide, N-(2,6-dimethylphenyl)maleimide, bis(4-maleimidophenyl)methane, 2,2-bis(4-(4-maleimidophenoxy)-phenyl)propane, bis(3,5-dimethyl-4-maleimidophenyl)methane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bis(3,5-diethyl-4-maleimidophenyl)methane, polyphenylmethane bismaleimide, bismaleimide containing biphenyl structure and polymaleimide.

[0088] The present invention also provides a method for preparing the modified bismaleimide resin as described above, comprising the following steps:

[0089] The modifier is mixed with bismaleimide resin and reacted at 100°C to 150°C.

[0090] In one embodiment, the reaction time is 60 min to 120 min.

[0091] In one embodiment, the preparation method of the modified bismaleimide resin comprises the following steps:

[0092] First, the fluorine-containing allyl compound represented by formula (I) is heated to a molten state, and the bismaleimide resin is added, and the reaction is prepolymerized at 100-150° C. for 60-120 minutes and then cooled to room temperature to obtain the modified bismaleimide resin.

[0093] The present invention also provides the application of the modified bismaleimide resin as described above, and the technical scheme is as follows:

[0094] A resin composition comprising the following components in parts by weight:

[0095] 30 to 80 parts of the modified bismaleimide resin as described above;

[0096] 20 to 60 parts of cyanate resin; and

[0097] 5 to 20 parts of functional resin.

[0098] The modified bismaleimide resin is compounded with a cyanate resin and a functional resin to prepare a resin composition, so that the resin composition also has excellent heat resistance, low water absorption, high modulus and excellent dielectric properties.

[0099] It can be understood that in the present invention, the resin composition contains 30 to 80 parts of modified bismaleimide resin, by mass, including but not limited to 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts and 80 parts, preferably 40 to 60 parts.

[0100] It can be understood that in the present invention, the resin composition contains 20 to 60 parts of cyanate ester resin by mass, including but not limited to 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts and 60 parts, preferably 30 to 50 parts.

[0101] In one embodiment, the cyanate ester resin is selected from one or more of bisphenol A cyanate ester resin, phenolic cyanate ester resin, bisphenol F cyanate ester resin, multifunctional cyanate ester resin, bisphenol M cyanate ester resin, bisphenol E cyanate ester resin and dicyclopentadiene bisphenol cyanate ester resin.

[0102] It can be understood that in the present invention, the resin composition contains 5 to 20 parts of functional resin by mass, including but not limited to 5, 8, 10, 12, 15, 16, 18 and 20 parts, preferably 5 to 15 parts.

[0103] In one embodiment, the functional resin is selected from one or more of epoxy resin, benzoxazine and polybutadiene.

[0104] In one embodiment, the epoxy resin is selected from one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, naphthalene epoxy resin, DCPD epoxy resin, biphenyl epoxy resin, anthracene epoxy resin, multifunctional epoxy resin and hydrogenated epoxy resin.

[0105] In one embodiment, the benzoxazine is selected from one or more of bisphenol A benzoxazine, bisphenol F benzoxazine, DCPD benzoxazine, phenolphthalein benzoxazine, phosphorus-containing benzoxazine, ODA benzoxazine, allyl benzoxazine and diamine benzoxazine.

[0106] In one embodiment, the polybutadiene preferably has a number average molecular weight of 1000 g / mol-5000 g / mol.

[0107] In one embodiment, the resin composition further comprises one or more of a flame retardant, a filler, a curing accelerator, a coupling agent and a toughening agent.

[0108] In the present invention, the fluorine-containing allyl compound represented by formula (I) of the present invention is used. Under the synergistic flame retardant effect of fluorine and nitrogen, a small amount of flame retardant is added to achieve the UL94V0 flame retardant grade, thereby avoiding the negative problems caused by adding a large amount of flame retardant in the traditional way.

[0109] In one embodiment, the resin composition includes 5 to 20 parts of flame retardant by weight, including but not limited to 5, 8, 10, 12, 15, 16, 18 and 20 parts, preferably 5 to 10 parts.

[0110] In one embodiment, the flame retardant is selected from one or more of decabromodiphenylethane, tetrabromobisphenol A, brominated epoxy resin, phosphorus-containing epoxy resin, phosphorus-containing phenolic resin, phosphazene compound, phosphate ester compound and phosphorus-containing cyanate ester.

[0111] In one embodiment, the resin composition includes 0 to 40 parts of filler, by mass, including but not limited to 0, 0.01, 0.1, 1, 2, 5, 8, 10, 12, 15, 16, 18, 20, 25, 30, 35 and 40 parts, preferably 0.1 to 40 parts, and more preferably 10 to 30 parts.

[0112] In one embodiment, the filler is selected from one or more of zirconium vanadate, zirconium tungstate, hafnium tungstate, glass-ceramics, eucryptite, silica (spherical, composite and molten), quartz, mica powder, titanium dioxide, magnesium oxide, magnesium hydroxide, talc, aluminum oxide, silicon carbide, boron nitride, aluminum nitride, molybdenum oxide, barium sulfate, zinc molybdate, zinc borate, zinc stannate, zinc oxide, strontium titanate, barium titanate, calcium titanate, clay and kaolin.

[0113] In one embodiment, the curing accelerator is selected from one or more of tertiary amine accelerators, imidazole accelerators, peroxide accelerators, organic phosphorus accelerators and transition metal carboxylate accelerators.

[0114] In one embodiment, the coupling agent is selected from one or more of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, a metal composite coupling agent, a phosphate coupling agent and a borate coupling agent.

[0115] In one embodiment, the toughening agent is selected from one or more of styrene-butadiene rubber, phenolic resin, nitrile rubber and polyurethane.

[0116] In one embodiment, the resin composition comprises the following components in parts by weight:

[0117]

[0118] In one embodiment, the resin composition comprises the following components in parts by weight:

[0119]

[0120] In one embodiment, the resin composition comprises the following components in parts by weight:

[0121]

[0122]

[0123] The present invention also provides a prepreg, comprising the modified bismaleimide resin as described above, or the resin composition as described above.

[0124] The present invention also provides a method for preparing the prepreg as described above, comprising the following steps:

[0125] The resin composition is covered on the surface of the reinforcing material by an impregnation method and heated to semi-solidification to obtain a prepreg.

[0126] The process parameters of the semi-curing are: heating to a constant temperature of 150° C. to 250° C. for 2 min to 10 min.

[0127] The reinforcing material is an inorganic fiber material or an organic fiber material, and the inorganic fiber reinforcing material includes but is not limited to glass fiber (including different types such as E, NE, D, S, T, etc.), carbon fiber, silicon carbide fiber, asbestos fiber, etc. The organic fiber reinforcing material includes but is not limited to nylon, ultra-high molecular weight polyethylene fiber, aramid fiber, polyimide fiber, polyester fiber, cotton fiber, etc.

[0128] The present invention also provides a laminated board, comprising the modified bismaleimide resin as described above, or the resin composition as described above, or the prepreg as described above.

[0129] In one embodiment, the laminate further includes at least one layer of metal foil located on one side or both sides of the prepreg.

[0130] The present invention also provides a method for preparing the laminate as described above, comprising the following steps:

[0131] Several of the above-mentioned prepregs are laminated.

[0132] In one embodiment, the lamination process parameters are: temperature 150°C to 300°C, pressure 10kgf / cm 2 ~30kgf / cm 2 , under the condition of vacuum degree <2kPa, hot pressing is carried out for 200min~400min.

[0133] It can be understood that the “several prepregs” refers to at least one prepreg.

[0134] It is understandable that during lamination, a plurality of the prepregs, ie, one side or both sides of the laminated body may be coated with metal copper foil, and then laminated to obtain a laminated board clad with metal copper foil.

[0135] In one embodiment, the thickness of the metal copper foil is 3μm to 105μm, including but not limited to 3μm, 5μm, 8μm, 10μm, 15μm, 18μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, 75μm, 80μm, 85μm, 90μm, 95μm, 100μm and 105μm.

[0136] The present invention also provides a printed circuit board, comprising the modified bismaleimide resin as described above, or the resin composition as described above, or the prepreg as described above, or the laminate as described above.

[0137] The following is a specific example part (the following examples do not contain other unspecified components except inevitable impurities unless otherwise specified).

[0138] (1) Raw materials description:

[0139] The following raw materials can be purchased from commercial products:

[0140] Bismaleimide resin-1 can be purchased from KI Chemicals, model number BMI-80;

[0141] Bismaleimide resin-2 can be purchased from Yamato Chemical Industry Co., Ltd. under the model number BMI-5100.

[0142] Bisphenol A cyanate ester is available from Lonza Group under the model number BA-230S.

[0143] 2,2'-Diallyl bisphenol A can be purchased from Honghu Shuangma Resin Factory;

[0144] 2,2'-Diallyl bisphenol S can be purchased from Nippon Kayaku, model number ARM019;

[0145] Bisphenol A bisallyl ether can be purchased from Honghu Shuangma Resin Factory.

[0146] DCPD-type benzoxazine can be purchased from Huntsman under the model number LPY 11051;

[0147] DCPD type epoxy resin can be purchased from Nippon Kayaku, model number XD-1000.

[0148] The flame retardant can be purchased from Daba Chemical, model number PX200.

[0149] Spherical silica can be purchased from Yaduma, model number SC6500-SXD.

[0150] 2-Methylimidazole can be purchased from Shikoku Chemical.

[0151] (2) Synthesis example:

[0152] The preparation steps of the fluorine-containing allyl compound represented by formula (I) are as follows:

[0153] 1. Weigh hexafluorobisphenol AF (0.4 mol, 134.5 g) and place it in a three-necked bottle. Measure 300 mL of acetone and stir to completely dissolve it. Weigh anhydrous potassium carbonate (0.1 mol, 138.2 g) and potassium iodide (3 wt.% hexafluorobisphenol AF, 4.035 g) and place them in the bottle. Adjust the speed to suspend the solid in the solution.

[0154] 2. Add allyl bromide (0.1 mol, 120.98 g) in a nitrogen atmosphere, and stir and reflux under nitrogen atmosphere at 60°C for 26 hours. Finally, the reaction status was detected by spot plate;

[0155] 3. After the reaction is completed, remove the potassium carbonate and potassium iodide solids by suction filtration; remove the acetone from the liquid by vacuum distillation;

[0156] 4. The liquid obtained after reduced pressure distillation is purified by column chromatography (eluent: pure petroleum ether), and the petroleum ether is removed by rotary evaporation to obtain a colorless oily liquid, which is dried to obtain a fluorine-containing allyl compound represented by formula (I), named 2,2-bis(4-allyloxyphenyl)hexafluoropropane, which is used as a modifier for bismaleimide resin in the following examples.

[0157] Embodiment 1:

[0158] This embodiment provides a modified bismaleimide resin and a preparation method thereof, a resin composition and a preparation method thereof, a prepreg and a preparation method thereof, and a laminate and a preparation method thereof, as follows:

[0159] (1) First, 70 parts of 2,2-bis(4-allyloxyphenyl)hexafluoropropane and 100 parts of bismaleimide resin-1 were mixed evenly, and prepolymerized at 120° C. for 90 minutes and then cooled to room temperature to obtain modified bismaleimide resin A.

[0160] (2) 40 parts of the modified bismaleimide resin A, 40 parts of bisphenol A cyanate resin and 10 parts of DCPD epoxy resin are dissolved in a mixed solvent of butanone, toluene and propylene glycol methyl ether, wherein butanone, toluene and propylene glycol methyl ether are mixed in a mass ratio of 1:1:1. Under stirring conditions, 10 parts of spherical silica, 10 parts of flame retardant and 3 parts of 2-methylimidazole are added, and stirring is continued to obtain a uniform glue solution, i.e., a modified bismaleimide resin composition.

[0161] (3) 2116 glass fiber cloth (basic weight 105g / m 2 ) was impregnated with the modified bismaleimide resin composition, and baked in a hot air circulation oven at 180° C. for 3 min to obtain a prepreg with a resin content of 50%.

[0162] (4) Six prepregs were stacked, and a 18 μm thick electrolytic copper foil was covered on each of the upper and lower surfaces of the stack. The stack was placed in a programmable temperature and pressure controlled vacuum press and heated to 30 kgf / cm2 in a vacuum state. 2 Under pressure, a 0.6mm thick copper-clad laminate was produced after curing at 220℃*3h.

[0163] Embodiment 2:

[0164] This embodiment provides a modified bismaleimide resin and a preparation method thereof, a resin composition and a preparation method thereof, a prepreg and a preparation method thereof, and a laminate and a preparation method thereof, as follows:

[0165] (1) First, 70 parts of 2,2-bis(4-allyloxyphenyl)hexafluoropropane and 100 parts of bismaleimide resin-1 were mixed evenly, and prepolymerized at 120° C. for 90 minutes and then cooled to room temperature to obtain modified bismaleimide resin A.

[0166] (2) 50 parts of the modified bismaleimide resin A, 50 parts of bisphenol A cyanate resin and 15 parts of DCPD epoxy resin are dissolved in a mixed solvent of butanone, toluene and propylene glycol methyl ether, wherein butanone, toluene and propylene glycol methyl ether are mixed in a mass ratio of 1:1:1. Under stirring conditions, 30 parts of spherical silica, 5 parts of flame retardant and 5 parts of 2-methylimidazole are added, and stirring is continued to obtain a uniform glue solution, i.e., a modified bismaleimide resin composition.

[0167] (3) 2116 glass fiber cloth (basic weight 105g / m 2 ) was impregnated with the modified bismaleimide resin composition, and baked in a hot air circulation oven at 180° C. for 3 min to obtain a prepreg with a resin content of 50%.

[0168] (4) Six prepregs were stacked, and a 18 μm thick electrolytic copper foil was covered on each of the upper and lower surfaces of the stack. The stack was placed in a programmable temperature and pressure controlled vacuum press and heated to 30 kgf / cm2 in a vacuum state. 2 Under pressure, a 0.6mm thick copper-clad laminate was produced after curing at 220℃*3h.

[0169] Embodiment 3:

[0170] This embodiment provides a modified bismaleimide resin and a preparation method thereof, a resin composition and a preparation method thereof, a prepreg and a preparation method thereof, and a laminate and a preparation method thereof, as follows:

[0171] (1) First, 70 parts of 2,2-bis(4-allyloxyphenyl)hexafluoropropane and 100 parts of bismaleimide resin-1 were mixed evenly, and prepolymerized at 120° C. for 90 minutes and then cooled to room temperature to obtain modified bismaleimide resin A.

[0172] (2) 60 parts of the modified bismaleimide resin A, 30 parts of bisphenol A cyanate resin and 5 parts of DCPD epoxy resin are dissolved in a mixed solvent of butanone, toluene and propylene glycol methyl ether, wherein butanone, toluene and propylene glycol methyl ether are mixed in a mass ratio of 1:1:1. Under stirring conditions, 20 parts of spherical silica, 8 parts of flame retardant and 1 part of 2-methylimidazole are added, and stirring is continued to obtain a uniform glue solution, i.e., a modified bismaleimide resin composition.

[0173] (3) 2116 glass fiber cloth (basic weight 105g / m 2 ) was impregnated with the modified bismaleimide resin composition, and baked in a hot air circulation oven at 180° C. for 3 min to obtain a prepreg with a resin content of 50%.

[0174] (4) Six prepregs were stacked, and a 18 μm thick electrolytic copper foil was covered on each of the upper and lower surfaces of the stack. The stack was placed in a programmable temperature and pressure controlled vacuum press and heated to 30 kgf / cm2 in a vacuum state. 2 Under pressure, a 0.6mm thick copper-clad laminate was produced after curing at 220℃*3h.

[0175] Embodiment 4:

[0176] This embodiment provides a modified bismaleimide resin and a preparation method thereof, a resin composition and a preparation method thereof, a prepreg and a preparation method thereof, and a laminate and a preparation method thereof, as follows:

[0177] (1) First, 50 parts of 2,2-bis(4-allyloxyphenyl)hexafluoropropane, 20 parts of 2,2'-diallylbisphenol A and 100 parts of bismaleimide resin-1 were mixed uniformly, and prepolymerized at 120° C. for 90 minutes and then cooled to room temperature to obtain modified bismaleimide resin B.

[0178] (2) 50 parts of the modified bismaleimide resin B, 50 parts of bisphenol A cyanate resin and 15 parts of DCPD epoxy resin are dissolved in a mixed solvent of butanone, toluene and propylene glycol methyl ether, wherein butanone, toluene and propylene glycol methyl ether are mixed in a mass ratio of 1:1:1. Under stirring conditions, 30 parts of spherical silica, 5 parts of flame retardant and 5 parts of 2-methylimidazole are added, and stirring is continued to obtain a uniform glue solution, i.e., a modified bismaleimide resin composition.

[0179] (3) 2116 glass fiber cloth (basic weight 105g / m 2 ) was impregnated with the modified bismaleimide resin composition, and baked in a hot air circulation oven at 180° C. for 3 min to obtain a prepreg with a resin content of 50%.

[0180] (4) Six prepregs were stacked, and a 18 μm thick electrolytic copper foil was covered on each of the upper and lower surfaces of the stack. The stack was placed in a programmable temperature and pressure controlled vacuum press and heated to 30 kgf / cm2 in a vacuum state. 2 Under pressure, a 0.6mm thick copper-clad laminate was produced after curing at 220℃*3h.

[0181] Embodiment 5:

[0182] This embodiment provides a modified bismaleimide resin and a preparation method thereof, a resin composition and a preparation method thereof, a prepreg and a preparation method thereof, and a laminate and a preparation method thereof, as follows:

[0183] (1) First, 70 parts of 2,2-bis(4-allyloxyphenyl)hexafluoropropane and 100 parts of bismaleimide resin-1 were mixed evenly, and prepolymerized at 120° C. for 90 minutes and then cooled to room temperature to obtain modified bismaleimide resin A.

[0184] (2) 50 parts of the modified bismaleimide resin A, 50 parts of bisphenol A cyanate resin and 15 parts of DCPD benzoxazine are dissolved in a mixed solvent of butanone, toluene and propylene glycol methyl ether, wherein butanone, toluene and propylene glycol methyl ether are mixed in a mass ratio of 1:1:1. Under stirring conditions, 30 parts of spherical silica, 5 parts of flame retardant and 5 parts of 2-methylimidazole are added, and stirring is continued to obtain a uniform glue solution, i.e., a modified bismaleimide resin composition.

[0185] (3) 2116 glass fiber cloth (basic weight 105g / m 2 ) was impregnated with the modified bismaleimide resin composition, and baked in a hot air circulation oven at 180° C. for 3 min to obtain a prepreg with a resin content of 50%.

[0186] (4) Six prepregs were stacked, and a 18 μm thick electrolytic copper foil was covered on each of the upper and lower surfaces of the stack. The stack was placed in a programmable temperature and pressure controlled vacuum press and heated to 30 kgf / cm2 in a vacuum state. 2 Under pressure, a 0.6mm thick copper-clad laminate was produced after curing at 220℃*3h.

[0187] Embodiment 6:

[0188] This embodiment provides a modified bismaleimide resin and a preparation method thereof, a resin composition and a preparation method thereof, a prepreg and a preparation method thereof, and a laminate and a preparation method thereof, as follows:

[0189] (1) First, 70 parts of 2,2-bis(4-allyloxyphenyl)hexafluoropropane and 100 parts of bismaleimide resin-2 were mixed evenly, and prepolymerized at 120° C. for 90 minutes and then cooled to room temperature to obtain modified bismaleimide resin C.

[0190] (2) 50 parts of the modified bismaleimide resin C, 50 parts of bisphenol A cyanate resin and 15 parts of DCPD epoxy resin are dissolved in a mixed solvent of butanone, toluene and propylene glycol methyl ether, wherein butanone, toluene and propylene glycol methyl ether are mixed in a mass ratio of 1:1:1. Under stirring conditions, 30 parts of spherical silica, 5 parts of flame retardant and 5 parts of 2-methylimidazole are added, and stirring is continued to obtain a uniform glue solution, i.e., a modified bismaleimide resin composition.

[0191] (3) 2116 glass fiber cloth (basic weight 105g / m2 ) was impregnated with the modified bismaleimide resin composition, and baked in a hot air circulation oven at 180° C. for 3 min to obtain a prepreg with a resin content of 50%.

[0192] (4) Six prepregs were stacked, and a 18 μm thick electrolytic copper foil was covered on each of the upper and lower surfaces of the stack. The stack was placed in a programmable temperature and pressure controlled vacuum press and heated to 30 kgf / cm2 in a vacuum state. 2 Under pressure, a 0.6mm thick copper-clad laminate was produced after curing at 220℃*3h.

[0193] Comparative Example 1:

[0194] This comparative example provides a modified bismaleimide resin and a preparation method thereof, a resin composition and a preparation method thereof, a prepreg and a preparation method thereof, and a laminate and a preparation method thereof, as follows:

[0195] (1) First, 70 parts of 2,2'-diallyl bisphenol A The mixture was mixed evenly with 100 parts of bismaleimide resin, prepolymerized at 120° C. for 90 minutes, and then cooled to room temperature to obtain modified bismaleimide resin D.

[0196] (2) 50 parts of the modified bismaleimide resin D, 50 parts of bisphenol A cyanate resin and 15 parts of DCPD epoxy resin are dissolved in a mixed solvent of butanone, toluene and propylene glycol methyl ether, wherein butanone, toluene and propylene glycol methyl ether are mixed in a mass ratio of 1:1:1. Under stirring conditions, 30 parts of spherical silica, 5 parts of flame retardant and 5 parts of 2-methylimidazole are added, and stirring is continued to obtain a uniform glue solution, i.e., a modified bismaleimide resin composition.

[0197] (3) 2116 glass fiber cloth (basic weight 105g / m 2 ) was impregnated with the modified bismaleimide resin composition, and baked in a hot air circulation oven at 180° C. for 3 min to obtain a prepreg with a resin content of 50%.

[0198] (4) Six prepregs were stacked, and a 18 μm thick electrolytic copper foil was covered on each of the upper and lower surfaces of the stack. The stack was placed in a programmable temperature and pressure controlled vacuum press and heated to 30 kgf / cm2 in a vacuum state. 2 Under pressure, a 0.6mm thick copper-clad laminate was produced after curing at 220℃*3h.

[0199] Comparative Example 2:

[0200] This comparative example provides a modified bismaleimide resin and a preparation method thereof, a resin composition and a preparation method thereof, a prepreg and a preparation method thereof, and a laminate and a preparation method thereof, as follows:

[0201] (1) First, 70 parts of 2,2'-diallyl bisphenol The mixture was mixed evenly with 100 parts of bismaleimide resin-1, and prepolymerized at 120° C. for 90 minutes, and then cooled to room temperature to obtain modified bismaleimide prepolymer E.

[0202] (2) 50 parts of the modified bismaleimide resin E, 50 parts of bisphenol A cyanate resin and 15 parts of DCPD epoxy resin are dissolved in a mixed solvent of butanone, toluene and propylene glycol methyl ether, wherein butanone, toluene and propylene glycol methyl ether are mixed in a mass ratio of 1:1:1. Under stirring conditions, 30 parts of spherical silica, 5 parts of flame retardant and 5 parts of 2-methylimidazole are added, and stirring is continued to obtain a uniform glue solution, i.e., a modified bismaleimide resin composition.

[0203] (3) 2116 glass fiber cloth (basic weight 105g / m 2 ) was impregnated with the modified bismaleimide resin composition, and baked in a hot air circulation oven at 180° C. for 3 min to obtain a prepreg with a resin content of 50%.

[0204] (4) Six prepregs were stacked, and a 18 μm thick electrolytic copper foil was covered on each of the upper and lower surfaces of the stack. The stack was placed in a programmable temperature and pressure controlled vacuum press and heated to 30 kgf / cm2 in a vacuum state. 2 Under pressure, a 0.6mm thick copper-clad laminate was produced after curing at 220℃*3h.

[0205] Comparative Example 3:

[0206] This comparative example provides a modified bismaleimide resin and a preparation method thereof, a resin composition and a preparation method thereof, a prepreg and a preparation method thereof, and a laminate and a preparation method thereof, as follows:

[0207] (1) First, 70 parts of bisphenol A bisallyl ether The mixture was mixed evenly with 100 parts of bismaleimide resin-1, prepolymerized at 120° C. for 90 minutes, and then cooled to room temperature to obtain modified bismaleimide resin F.

[0208] (2) 50 parts of the modified bismaleimide resin F, 50 parts of bisphenol A cyanate resin and 15 parts of DCPD epoxy resin are dissolved in a mixed solvent of butanone, toluene and propylene glycol methyl ether, wherein butanone, toluene and propylene glycol methyl ether are mixed in a mass ratio of 1:1:1. Under stirring conditions, 30 parts of spherical silica, 5 parts of flame retardant and 5 parts of 2-methylimidazole are added, and stirring is continued to obtain a uniform glue solution, i.e., a modified bismaleimide resin composition.

[0209] (3) 2116 glass fiber cloth (basic weight 105g / m 2 ) was impregnated with the modified bismaleimide resin composition, and baked in a hot air circulation oven at 180° C. for 3 min to obtain a prepreg with a resin content of 50%.

[0210] (4) Six prepregs were stacked, and a 18 μm thick electrolytic copper foil was covered on each of the upper and lower surfaces of the stack. The stack was placed in a programmable temperature and pressure controlled vacuum press and heated to 30 kgf / cm2 in a vacuum state. 2 Under pressure, a 0.6mm thick copper-clad laminate was produced after curing at 220℃*3h.

[0211] Comparative Example 4:

[0212] This comparative example provides a resin composition and a preparation method thereof, a prepreg and a preparation method thereof, a laminate and a preparation method thereof, which are specifically as follows:

[0213] (1) 50 parts of bismaleimide resin-1, 50 parts of bisphenol A cyanate resin and 15 parts of DCPD epoxy resin are dissolved in a mixed solvent of butanone, toluene and propylene glycol methyl ether, wherein butanone, toluene and propylene glycol methyl ether are mixed in a mass ratio of 1:1:1. Under stirring conditions, 30 parts of spherical silica, 5 parts of flame retardant and 5 parts of 2-methylimidazole are added, and stirring is continued to obtain a uniform glue solution, i.e., a bismaleimide resin composition.

[0214] (2) 2116 glass fiber cloth (basic weight 105g / m 2 ) was impregnated with the above-mentioned bismaleimide resin composition, and baked in a hot air circulation oven at 180° C. for 3 min to obtain a prepreg with a resin content of 50%.

[0215] (3) Six prepreg sheets were stacked, and a 18 μm thick electrolytic copper foil was covered on each of the upper and lower surfaces of the stacked body. The stacked body was placed in a programmable temperature and pressure controlled vacuum press and heated to 30 kgf / cm2 in a vacuum state. 2 Under pressure, a 0.6mm thick copper-clad laminate was produced after curing at 220℃*3h.

[0216] Comparative Example 5:

[0217] This comparative example provides a modified bismaleimide resin and a preparation method thereof, a resin composition and a preparation method thereof, a prepreg and a preparation method thereof, and a laminate and a preparation method thereof, as follows:

[0218] (1) First, 70 parts of 2,2-bis(4-allyloxyphenyl)hexafluoropropane and 100 parts of bismaleimide resin-1 were mixed evenly, and prepolymerized at 120° C. for 90 minutes and then cooled to room temperature to obtain modified bismaleimide resin A.

[0219] (2) 90 parts of the modified bismaleimide resin A, 30 parts of bisphenol A cyanate resin and 5 parts of DCPD epoxy resin are dissolved in a mixed solvent of butanone, toluene and propylene glycol methyl ether, wherein butanone, toluene and propylene glycol methyl ether are mixed in a mass ratio of 1:1:1. Under stirring conditions, 20 parts of spherical silica, 8 parts of flame retardant and 1 part of 2-methylimidazole are added, and stirring is continued to obtain a uniform glue solution, i.e., a modified bismaleimide resin composition.

[0220] (3) 2116 glass fiber cloth (basic weight 105g / m 2 ) was impregnated with the modified bismaleimide resin composition, and baked in a hot air circulation oven at 180° C. for 3 min to obtain a prepreg with a resin content of 50%.

[0221] (4) Six prepregs were stacked, and a 18 μm thick electrolytic copper foil was covered on each of the upper and lower surfaces of the stack. The stack was placed in a programmable temperature and pressure controlled vacuum press and heated to 30 kgf / cm2 in a vacuum state. 2 Under pressure, a 0.6mm thick copper-clad laminate was produced after curing at 220℃*3h.

[0222] 1) The components of the resin composition in the above examples and comparative examples are shown in Table 1 below:

[0223] Table 1

[0224]

[0225]

[0226] 2) The copper-clad laminates prepared in Examples 1-6 and Comparative Examples 1-5 were tested for performance as follows:

[0227] (1) Peel strength: The test method is carried out in accordance with IPC-TM-650 2.4.8;

[0228] (2) Glass transition temperature (Tg): Tested according to IPC-TM650 2.4.25D;

[0229] (3) Thermal decomposition temperature (Td): tested according to IPC-TM650 2.4.24.6;

[0230] (4) Elastic modulus: tested according to GB / T 22315-2008;

[0231] (5) Flame retardant: tested according to IPC-TM650 2.3.10;

[0232] (6) Water absorption: Tested according to IPC-TM650 2.6.2.1;

[0233] (7)Dk / Df: Tested according to IPC-TM650 2.5.5.2.

[0234] The test results are shown in Table 2:

[0235] Table 2

[0236]

[0237] As shown in Table 2, the peel strength, heat resistance, water absorption, elastic modulus, dielectric properties and flame retardant properties of Examples 1 to 6 within the scope of protection of the present invention are excellent, and the performance is greatly improved compared to Comparative Examples 1 to 3 using traditional modifiers. Comparative Example 4 is unmodified bismaleimide, and its performance is the worst, indicating that unmodified bismaleimide is difficult to use. In conjunction with Comparative Example 5, it can be seen that the addition amount of each raw material is very important for the performance of the copper-clad laminate.

[0238] In addition, because the modifier in the present invention contains fluorine element, it can work synergistically with nitrogen element to greatly improve the flame retardant performance, and only a small amount of flame retardant needs to be added to achieve the UL94V0 grade.

[0239] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0240] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A resin composition, characterized in that The composition includes the following components in parts by weight: 40 to 60 parts of modified bismaleimide resin; 30 to 50 parts of cyanate resin; and 5 to 15 parts of functional resin; The raw materials of the modified bismaleimide resin include a modifier and a bismaleimide resin; the modifier includes a fluorine-containing allyl compound, and the fluorine-containing allyl compound has a structure shown in formula (I):

2. The resin composition according to claim 1, characterized in that The preparation method of the fluorine-containing allyl compound comprises the following steps: Mixing hexafluorobisphenol AF, a base and a catalyst in a solvent to prepare a suspension; The suspension is mixed with allyl bromide and reacted.

3. The resin composition according to claim 2, characterized in that The molar ratio of hexafluorobisphenol AF, alkali and propylene bromide is 1:(0.2-4):(0.2-6); and / or The base is one or more selected from the group consisting of potassium carbonate, cesium carbonate, sodium carbonate, potassium hydroxide, sodium hydroxide, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and tetrabutylammonium hydroxide; and / or The catalyst is selected from one or more of potassium iodide, cesium iodide and sodium iodide.

4. The resin composition according to claim 1, characterized in that The mass ratio of the fluorine-containing allyl compound to the bismaleimide resin is (0.5-1):

1.

5. The resin composition according to claim 1, characterized in that The modifier further comprises one or more of 2,2'-diallyl bisphenol A, 2,2'-diallyl bisphenol S, 2,2'-diallyl bisphenol F and bisphenol A bisallyl ether.

6. The resin composition according to claim 1, characterized in that The bismaleimide resin contains two or more maleimide groups.

7. The resin composition according to claim 1, characterized in that The monomer of the bismaleimide resin is selected from one or more of N-phenylmaleimide, N-(2-methylphenyl)maleimide, N-(4-methylphenyl)maleimide, N-(2,6-dimethylphenyl)maleimide, bis(4-maleimidophenyl)methane, 2,2-bis(4-(4-maleimidophenoxy)-phenyl)propane, bis(3,5-dimethyl-4-maleimidophenyl)methane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bis(3,5-diethyl-4-maleimidophenyl)methane, polyphenylmethane bismaleimide, bismaleimide containing biphenyl structure and polymaleimide.

8. The resin composition according to claim 1, characterized in that The preparation method of the modified bismaleimide resin comprises the following steps: The modifier is mixed with bismaleimide resin and reacted at 100°C to 150°C.

9. The resin composition according to claim 1, characterized in that The cyanate resin is selected from one or more of bisphenol A cyanate resin, phenolic cyanate resin, bisphenol F cyanate resin, multifunctional cyanate resin, bisphenol M cyanate resin, bisphenol E cyanate resin and dicyclopentadiene bisphenol cyanate resin.

10. The resin composition according to claim 1, characterized in that The functional resin is selected from one or more of epoxy resin, benzoxazine and polybutadiene.

11. The resin composition according to any one of claims 1 to 10, characterized in that It also includes one or more of a flame retardant, a filler, a curing accelerator, a coupling agent and a toughening agent.

12. The resin composition according to any one of claims 1 to 10, characterized in that The resin composition comprises 5 to 20 parts of a flame retardant and 0 to 40 parts of a filler in parts by mass.

13. The resin composition according to claim 12, characterized in that The flame retardant is one or more selected from the group consisting of decabromodiphenylethane, tetrabromobisphenol A, brominated epoxy resin, phosphorus-containing epoxy resin, phosphorus-containing phenolic resin, phosphazene compound, phosphate ester compound and phosphorus-containing cyanate; and / or The filler is selected from one or more of zirconium vanadate, zirconium tungstate, hafnium tungstate, microcrystalline glass, eucryptite, silicon dioxide, quartz, mica powder, titanium dioxide, magnesium oxide, magnesium hydroxide, talc, aluminum oxide, silicon carbide, boron nitride, aluminum nitride, molybdenum oxide, barium sulfate, zinc molybdate, zinc borate, zinc stannate, zinc oxide, strontium titanate, barium titanate, calcium titanate, clay and kaolin.

14. A prepreg, characterized in that: The resin composition comprising any one of claims 1 to 13.

15. A laminated board, characterized in that: The invention comprises the resin composition according to any one of claims 1 to 13, or the prepreg according to claim 14.

16. The laminate according to claim 15, characterized in that The laminate further comprises at least one layer of metal foil located on one side or both sides of the prepreg.

17. A printed circuit board, characterized in that: The invention comprises the resin composition according to any one of claims 1 to 13, or the prepreg according to claim 14, or the laminate according to claim 15 or 16.