A metal-based foam-loaded material and its preparation method and application
By using metal-based foam-supported materials as catalysts, the problems of low yield and poor stability of existing catalysts in catalyzing the reaction of CO2 and dimethylamine are solved, and DMF is efficiently prepared and suitable for actual production. The materials prepared by combustion method have Excellent catalytic performance.
Patent Information
- Application Number
- CN202111536218.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-12-15
AI Technical Summary
When the existing catalysts catalyze the reaction of CO2 and dimethylamine to prepare DMF, the yield is low and the stability is poor, making it difficult to apply to actual production, and the homogeneous catalysts used are expensive and difficult to promote.
Using metal-based foam-supported materials as catalysts, the metal oxide precursor and the combustion agent are dissolved and immersed into the metal-based foam carrier, and then prepared by calcination to form a metal-based matrix of metal elements such as Pd, Ru, Cu, Co and Ni. Foam-supported material, used as a catalyst for the reaction of CO2, H2 and dimethylamine.
It improves the yield of DMF and the stability of the catalyst, is suitable for practical production applications, and the materials prepared by combustion have rich pores and small particle sizes, enhancing the specific surface area and catalytic properties.
Smart Images

Figure BDA0003412645940000081 
Figure BDA0003412645940000091 
Figure BDA0003412645940000101
Abstract
Description
Technical Field
[0001] The invention relates to the field of catalytic technology, and in particular to a metal-based foam-supported material and a preparation method and application thereof. Background Art
[0002] At present, the global annual carbon dioxide emissions are about 40 billion tons, of which 14% comes from land use and 86% comes from fossil energy use. The development of CO2 chemical conversion technology can not only reduce the CO2 content in the atmosphere but also bring considerable economic benefits.
[0003] N,N-dimethylformamide (DMF) is a widely used organic solvent, commonly used in the plastics, pharmaceutical and paint industries. The industrial synthesis method of DMF is mainly to directly react dimethylamine and carbon monoxide with sodium methoxide to produce DMF. In actual production, the sodium methoxide catalyst has extremely high requirements for the purity of the reaction raw materials, and a small amount of water will also cause the catalyst to be deactivated. In addition, byproducts such as monomethylformamide (MMF), dimethylacetamide (DMAC), formic acid, and salt substances such as sodium hydroxide, sodium formate, sodium bicarbonate, and sodium carbonate are produced during the reaction. The use of green CO2, dimethylamine, and hydrogen to prepare DMF through N-formylation reaction not only has important economic value but also has practical environmental significance. It is one of the effective ways to achieve carbon neutrality.
[0004] Patent US4269998 reported in 1981 that Raney Ni, Raney Cu, Raney Co and loaded precious metals were used as catalysts to catalyze the synthesis of DMF from CO2, H2 and dimethylamine, but the maximum yield was 37.2%; Liu et al. (Synthesis of dimethylformamide from CO2, H2 and dimethylamine over Cu / ZnO, Chemical Communication, 2010, 46, 5770-5772) used copper-loaded zinc oxide as a catalyst to catalyze the reaction of dimethylamine with CO2 and H2 to prepare DMF with a yield of 97%, but due to related technical problems such as the stability of the catalyst, this method is still in the experimental research stage. In 1970, Haynes et al. (Formamides from carbon dioxide, amines and hydrogen in the presence of metal complexes, Tetrahedron Lett., 11, 365-368) used a homogeneous catalyst Pd(CO3)[P(C6H5)3]2 to catalyze the synthesis of DMF from CO2, H2 and dimethylamine. However, some reports in recent years have used expensive homogeneous catalysts, which are difficult to apply to actual production. Summary of the invention
[0005] The purpose of the present invention is to provide a metal-based foam-supported material and a preparation method and application thereof. The metal-based foam-supported material provided by the present invention is used as a catalyst for catalyzing CO2 reaction to prepare DMF. Not only is the yield of DMF high, but the catalyst performance is stable and suitable for actual production.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The invention provides a metal-based foam-supported material, comprising a metal-based foam carrier and a metal oxide supported on the metal-based foam carrier; the metal element in the metal oxide is one or more of Pd, Ru, Cu, Co and Ni.
[0008] Preferably, the metal-based foam carrier includes foamed aluminum, foamed copper or foamed nickel.
[0009] Preferably, the mass of the metal element in the metal oxide is 0.1-10% of the mass of the metal-based foam-supported material.
[0010] The present invention provides a method for preparing the metal-based foam-supported material described in the above scheme, comprising the following steps:
[0011] Dissolving a metal oxide precursor and a combustion agent in water to obtain an impregnation solution; the combustion agent is urea, citric acid, glycine or ethylene glycol;
[0012] Impregnating the metal-based foam carrier into the impregnation solution, and then calcining the obtained impregnation system to obtain the metal-based foam supported material;
[0013] The metal oxide precursor is a soluble salt of a metal element; the metal element is one or more of Pd, Ru, Cu, Co and Ni.
[0014] Preferably, the molar ratio of the metal oxide precursor to the combustion agent is 1:0.8-3.
[0015] Preferably, the total mass concentration of the metal oxide precursor and the combustion agent in the impregnation solution is not less than 1.5%.
[0016] Preferably, the calcination is carried out in an air atmosphere; the calcination temperature is 500-800° C., and the holding time is 5-10 min.
[0017] Preferably, the immersion time is 2 to 6 hours.
[0018] The present invention provides the use of the metal-based foam-supported material described in the above scheme or the metal-based foam-supported material prepared by the preparation method described in the above scheme as a catalyst in catalyzing the reaction of CO2, H2 and dimethylamine to prepare N,N-dimethylformamide.
[0019] Preferably, the molar ratio of dimethylamine to CO2 is 1:1-10; the reaction pressure is 4-10 MPa, wherein the molar ratio of CO2 to H2 is 1:1-1.5; and the reaction temperature is 140-200°C.
[0020] The present invention provides a metal-based foam-supported material, comprising a metal-based foam carrier and a metal oxide supported on the metal-based foam carrier; the metal element in the metal oxide is one or more of Pd, Ru, Cu, Co and Ni. The present invention uses metal-based foam as a carrier and one or more of Pd, Ru, Cu, Co and Ni as an active component. The interaction between the carrier and the active component is strong, the active component is not easy to lose, and has better stability; the use of metal-based foam material as a carrier further increases the specific surface area of the metal-based foam-supported material, strengthens the mass transfer and diffusion effect of the reaction, and the metal-based foam-supported material of the present invention is used as a catalyst for catalyzing CO2 reaction to prepare DMF, which not only has a high yield of DMF, but also has stable catalyst performance and is suitable for actual production.
[0021] The present invention provides a method for preparing the metal-based foam-supported material described in the above scheme, comprising the following steps: dissolving a metal oxide precursor and a combustion agent in water to obtain an impregnation solution; the combustion agent is urea, citric acid, glycine or ethylene glycol; impregnating a metal-based foam carrier into the impregnation solution, and then calcining the obtained impregnation system to obtain a metal-based foam-supported material; the metal oxide precursor is a soluble salt of a metal element; the metal element is one or more of Pd, Ru, Cu, Co and Ni.
[0022] The present invention adopts a combustion method to prepare a metal-based foam-supported material, the combustion reaction is mild, and the obtained material has a uniform particle size. On the other hand, the combustion agent and the metal element can form a relatively stable complex to avoid the generation and precipitation of certain metal ions, thereby ensuring a small particle size. In addition, gases such as nitrogen or carbon dioxide are released during the combustion process, further avoiding the aggregation and growth of metals, and generating pores to increase the specific surface area. The metal-based foam-supported material prepared by the method of the present invention has abundant pores, small particle size, uniform particle size, and large specific surface area, which is conducive to improving the catalytic performance of the metal-based foam-supported material. In addition, by using the method of the present invention, the metal oxide and the carrier interact strongly, the active component is not easy to be lost, and has better stability. DETAILED DESCRIPTION
[0023] The invention provides a metal-based foam-supported material, comprising a metal-based foam carrier and a metal oxide supported on the metal-based foam carrier; the metal element in the metal oxide is one or more of Pd, Ru, Cu, Co and Ni.
[0024] The metal-based foam-supported material provided by the present invention comprises a metal-based foam carrier. In the present invention, the metal-based foam carrier preferably comprises foamed aluminum, foamed copper or foamed nickel. In the present invention, the specific gravity of the foamed nickel is preferably 0.2 to 0.5 g / cm 3 The porosity is preferably 80-95%. The present invention uses metal-based foam material as a carrier to increase the specific surface area of the metal-based foam-loaded material and strengthen the mass transfer and diffusion effect of the reaction.
[0025] The metal-based foam supported material provided by the present invention comprises a metal oxide supported on the metal-based foam support, wherein the metal element in the metal oxide is one or more of Pd, Ru, Cu, Co and Ni, preferably one or more of Pd, Ru, Cu and Ni, and more preferably one or more of Pd, Ru and Ni. In the present invention, when the metal element is a plurality of the above substances, the present invention has no special requirements for the ratio of each metal element, and any ratio is acceptable. The present invention has no special requirements for the specific type of the metal oxide, which is determined by the preparation method.
[0026] In the present invention, the mass of the metal element in the metal oxide is 0.1-10% of the mass of the metal-based foam-supported material, preferably 1-9%, and more preferably 2-8%.
[0027] In the present invention, the metal oxide is preferably located in the pores and on the surface of the metal-based foam support.
[0028] The present invention provides a method for preparing the metal-based foam-supported material described in the above scheme, comprising the following steps:
[0029] Dissolving a metal oxide precursor and a combustion agent in water to obtain an impregnation solution; the combustion agent is urea, citric acid, glycine or ethylene glycol;
[0030] impregnating the metal-based foam carrier into an impregnation solution, and then calcining the obtained impregnation system to obtain a metal-based foam-supported material;
[0031] The metal oxide precursor is a soluble salt of a metal element; the metal element is one or more of Pd, Ru, Cu, Co and Ni.
[0032] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0033] The invention dissolves the metal oxide precursor and the combustion agent into water to obtain the impregnation solution.
[0034] In the present invention, the combustion agent is urea, citric acid, glycine or ethylene glycol; the metal oxide precursor is a soluble salt of a metal element; and the metal element is one or more of Pd, Ru, Cu, Co and Ni.
[0035] In the present invention, the soluble salt is preferably a nitrate, an acetate or a chloride. In the present invention, the molar ratio of the metal oxide precursor to the combustion agent is preferably 1:0.8-3, more preferably 1:1-2.5, and further preferably 1:1.5-2.0.
[0036] In the present invention, the total mass concentration of the metal oxide precursor and the combustion agent in the impregnation solution is preferably not less than 1.5%, and more preferably 1.5-26%.
[0037] After obtaining the impregnation solution, the present invention impregnates the metal-based foam carrier into the impregnation solution, and then calcines the obtained impregnation system to obtain the metal-based foam supported material.
[0038] In the present invention, the impregnation time is preferably 2 to 6 hours, more preferably 3 to 5 hours. In the impregnation process of the present invention, the metal oxide precursor and the combustion agent are adsorbed into the pores and surface of the metal-based foam carrier.
[0039] In the present invention, the calcination temperature is preferably 500-800°C, more preferably 550-750°C, and further preferably 600-700°C; the holding time is preferably 5-10 min. The heating rate to the calcination temperature is preferably 1-5°C / min. In the present invention, the calcination is preferably carried out in an air atmosphere. In the calcination process of the present invention, the combustion agent acts as an oxidant and the metal oxide precursor acts as a reducing agent, and a combustion reaction occurs under air conditions to generate metal oxides loaded on a metal-based foam carrier, while generating gases such as nitrogen or carbon dioxide, producing more pores, and further increasing the specific surface area of the material.
[0040] The present invention provides the use of the metal-based foam-supported material described in the above scheme or the metal-based foam-supported material prepared by the preparation method described in the above scheme as a catalyst in catalyzing the reaction of CO2, H2 and dimethylamine to prepare N,N-dimethylformamide.
[0041] In the present invention, the molar ratio of dimethylamine and CO2 is preferably 1:1-10, more preferably 1:2-7, and further preferably 1:3-6; the pressure of the reaction is preferably 4-10 MPa, more preferably 6-8 MPa; wherein, the molar ratio of CO2 and H2 is preferably 1:1-1.5; and the temperature of the reaction is preferably 140-200°C.
[0042] In the present invention, the catalytic reaction of CO2, H2 and dimethylamine is preferably carried out in a high-pressure reactor or a fixed bed; when the reaction is carried out in a high-pressure reactor, the mass of the catalyst is preferably 2.0-10.0% of the mass of the dimethylamine raw material, and the reaction time is preferably 5-20 hours; when the reaction is carried out in a fixed bed, the mass space velocity of the dimethylamine is preferably 0.5-3.0 h -1 .
[0043] The metal-based foam-supported material provided by the present invention and its preparation method and application are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0044] Example 1 (Pd / foamed-Al 0.5wt%)
[0045] 23 mg of palladium nitrate (0.1 mmol) and 25 mg of citric acid (0.13 mmol) were weighed and dissolved in 3 mL of water. 2 g of sheet-shaped (0.5 cm*0.5 cm) aluminum foam was immersed in the solution for 2 hours. Then, it was placed in a muffle furnace and heated from room temperature to 500°C at a rate of 1°C / min, maintained for 5 min, cooled to room temperature, and taken out to obtain a Pd / foamed-Al catalyst, in which the Pd content was 0.5 wt%.
[0046] Example 2 (Ru / foamed-Al 1.0wt%)
[0047] 41.4 mg of ruthenium chloride (0.2 mmol) and 20 mg of glycine (0.26 mmol) were weighed and dissolved in 3 mL of water. 2 g of sheet-shaped (0.5 cm*0.5 cm) aluminum foam was immersed in the solution for 2 hours. Then, it was placed in a muffle furnace and heated from room temperature to 500°C at a rate of 1°C / min, maintained for 5 minutes, cooled to room temperature, and taken out to obtain a Ru / foamed-Al catalyst in which the Ru content was 0.5 wt%.
[0048] Example 3 (Pd-Cu / foamed-Al Pd0.5Cu5.0wt%)
[0049] 23 mg of palladium nitrate (0.1 mmol), 387 mg of copper nitrate (1.6 mmol) and 82 mg of urea (1.36 mmol) were weighed and dissolved in 3 mL of water, 2 g of sheet-shaped (0.5 cm*0.5 cm) aluminum foam was immersed in the solution for 4 hours, then placed in a muffle furnace, heated from room temperature to 600°C at a rate of 3°C / min, maintained for 8 min, cooled to room temperature, and taken out to obtain a Pd-Cu / foamed-Al catalyst, wherein the Pd content was 0.5 wt% and the Cu content was 5.0 wt%.
[0050] Example 4 (Pd-Ni / foamed-Al Pd0.5Ni4.7wt%)
[0051] 23 mg of palladium nitrate (0.1 mmol), 467 mg of nickel nitrate (1.6 mmol) and 82 mg of urea (1.36 mmol) were weighed and dissolved in 3 mL of water, 2 g of sheet-shaped (0.5 cm*0.5 cm) aluminum foam was immersed in the solution for 4 hours, then placed in a muffle furnace, heated from room temperature to 800°C at a rate of 3°C / min, maintained for 8 min, cooled to room temperature, and taken out to obtain a Pd-Ni / foamed-Al catalyst, wherein the Pd content was 0.5 wt% and the Ni content was 4.7 wt%.
[0052] Example 5 (Ru-Ni / foamed-Al Ru2.5Ni4.7wt%)
[0053] 104 mg of ruthenium chloride (0.5 mmol), 467 mg of nickel nitrate (1.6 mmol) and 130 mg of ethylene glycol (2.1 mmol) were weighed and dissolved in 3 mL of water. 2 g of sheet-shaped (0.5 cm*0.5 cm) aluminum foam was immersed in the solution for 6 hours. Then, it was placed in a muffle furnace and heated from room temperature to 800°C at a rate of 5°C / min, maintained for 8 min, cooled to room temperature, and taken out to obtain a Ru-Ni / foamed-Al catalyst, in which the Ru content was 2.5 wt% and the Ni content was 4.7 wt%.
[0054] Example 6 (Ru-Cu / foamed-Al Ru2.5Cu5.0wt%)
[0055] 104 mg of ruthenium chloride (0.5 mmol), 387 mg of copper nitrate (1.6 mmol) and 130 mg of ethylene glycol (2.1 mmol) were weighed and dissolved in 3 mL of water. 2 g of sheet-shaped (0.5 cm*0.5 cm) aluminum foam was immersed in the solution for 6 hours. Then, it was placed in a muffle furnace and heated from room temperature to 600°C at a rate of 5°C / min, maintained for 8 min, cooled to room temperature, and taken out to obtain a Ru-Cu / foamed-Al catalyst, in which the Ru content was 2.5 wt% and the Cu content was 5.0 wt%.
[0056] Example 7 (Cu / foamed-Al 10wt%)
[0057] 626 mg of copper acetate (3.13 mmol) and 235 mg of glycine (3.13 mmol) were weighed and dissolved in 3 mL of water, 2 g of sheet-shaped (0.5 cm*0.5 cm) aluminum foam was immersed in the solution for 6 hours, then placed in a muffle furnace, heated from room temperature to 500°C at a rate of 1°C / min, maintained for 10 min, cooled to room temperature, and taken out to obtain a Cu / foamed-Al catalyst, in which the Cu content was 10 wt%.
[0058] Example 8 (Pd-Cu / foamed-Ni Pd1.0Cu7.3wt%)
[0059] 46 mg of palladium nitrate (0.2 mmol), 557 mg of copper nitrate (2.3 mmol) and 150 mg of urea (2.5 mmol) were weighed and dissolved in 3 mL of water, 2 g of sheet-shaped (0.5 cm*0.5 cm) nickel foam was immersed in the solution for 5 hours, then placed in a muffle furnace, heated from room temperature to 700°C at a rate of 3°C / min, maintained for 6 min, cooled to room temperature, and taken out to obtain a Pd-Cu / foamed-Ni catalyst, wherein the Pd content was 1.0 wt% and the Cu content was 7.3 wt%.
[0060] Example 9 (Pd-Ni / foamed-Cu Pd1.0Ni6.7wt%)
[0061] 46 mg of palladium nitrate (0.2 mmol), 672 mg of nickel nitrate (2.3 mmol) and 150 mg of urea (2.5 mmol) were weighed and dissolved in 3 mL of water, 2 g of sheet-shaped (0.5 cm*0.5 cm) foamed copper was immersed in the solution for 5 hours, then placed in a muffle furnace, heated from room temperature to 700°C at a rate of 3°C / min, maintained for 6 min, cooled to room temperature, and taken out to obtain a Pd-Ni / foamed-Cu catalyst, wherein the Pd content was 1.0 wt% and the Ni content was 6.7 wt%.
[0062] Example 10 (Ru-Cu / foamed-Ni Ru2.52Cu7.31%)
[0063] 104 mg of ruthenium chloride (0.5 mmol), 336 mg of copper chloride (2.3 mmol) and 186 mg of ethylene glycol (3 mmol) were weighed and dissolved in 3 mL of water. 2 g of sheet-shaped (0.5 cm*0.5 cm) nickel foam was immersed in the solution for 5 hours. Then, it was placed in a muffle furnace and heated from room temperature to 700°C at a rate of 3°C / min, maintained for 6 min, cooled to room temperature, and taken out to obtain a Ru-Cu / foamed-Ni catalyst, in which the Ru content was 2.52 wt% and the Cu content was 7.31 wt%.
[0064] Example 11 (Ru-Ni / foamed-Cu Ru2.52Ni7.34%)
[0065] 104 mg of ruthenium chloride (0.5 mmol), 325 mg of nickel chloride (2.5 mmol) and 186 mg of ethylene glycol (3 mmol) were weighed and dissolved in 3 mL of water. 2 g of sheet-shaped (0.5 cm*0.5 cm) nickel foam was immersed in the solution for 5 hours. Then, it was placed in a muffle furnace and heated from room temperature to 700°C at a rate of 3°C / min, maintained for 6 min, cooled to room temperature, and taken out to obtain a Ru-Ni / foamed-Cu catalyst, in which the Ru content was 2.52 wt% and the Ni content was 7.34 wt%.
[0066] Example 12 (Ru-Co / foamed-Al Ru2.52Co7.36%)
[0067] 104 mg of ruthenium chloride (0.5 mmol), 325 mg of cobalt chloride (2.5 mmol) and 576 mg of citric acid (3 mmol) were weighed and dissolved in 3 mL of water. 2 g of sheet-shaped (0.5 cm*0.5 cm) aluminum foam was immersed in the solution for 5 hours. Then, it was placed in a muffle furnace and heated from room temperature to 700°C at a rate of 3°C / min, maintained for 6 minutes, cooled to room temperature, and taken out to obtain a Ru-Co / foamed-Al catalyst, in which the Ru content was 2.52 wt% and the Co content was 7.36 wt%.
[0068] Synthesis of DMF from CO2, H2 and dimethylamine
[0069] Application Examples 1 to 12
[0070] Weigh a certain amount of the supported catalysts prepared in Examples 1 to 12 respectively, add them into a 100 mL reactor with magnetic stirring, seal it, replace the air in the system with H2 three times, then inject 1.8 g of dimethylamine (40 mmol) with a double plunger pump, and then continue to charge with CO2 and H2 at the required pressure, heat and stir, and keep the temperature for a certain time after heating to the reaction temperature. Stop the reaction and cool to room temperature, and analyze the product.
[0071] Agilent 5977A / 7890BgC-MS gas mass spectrometer and Agilent 7890A (30m×0.25mm×0.33μm capillary column, hydrogen flame ionization detector) were used to qualitatively and quantitatively analyze the reaction products. The reaction conditions and results are shown in Table 1, where the yield of DMF was calculated based on dimethylamine.
[0072] Table 1 Conditions and results of catalytic DMF synthesis in Application Examples 1 to 12
[0073]
[0074]
[0075] It can be seen from the above experimental results that the supported catalyst prepared by the present invention can efficiently synthesize DMF.
[0076] Application Example 13
[0077] After the reaction of Application Example 4 is completed, the catalyst is recovered, cleaned, dried and reused. The reaction conditions are the same as those of Application Example 4. The experimental results are shown in Table 2.
[0078] Table 2 Experimental results of Pd-Ni / foamed-Al catalyst after multiple cycles of catalysis in Application Example 4
[0079] DMF yield / % Application Example 4 94.3 Second cycle 93.0 3rd cycle 92.8 4th cycle 92.6 5th cycle 91.9
[0080] It can be seen from the results in Table 2 that the supported catalyst material provided by the present invention is easy to recycle and reuse. After being reused for 5 times, the catalytic performance does not show obvious deactivation and has good stability.
[0081] Application Examples 14-17
[0082] The supported catalyst prepared in Examples 3 and 5 was used for a fixed bed reaction. The catalyst loading amount was 1 g and loaded into a Φ8 mm fixed bed reactor. After the fixed bed reaction system was purged with nitrogen, CO2 and H2 were connected, and the total pressure was adjusted to 6.5 MPa by a back pressure valve. The flow rates of each gas were controlled by a gas mass flowmeter, and dimethylamine was pumped into the reaction system at a controlled flow rate by a double plunger pump. The fixed bed was heated to 180° C. within 0.5 h, and the feed of each raw material was started at a specific space velocity after reaching the temperature. The fixed bed discharge port was connected to Agilent 8860 (hydrogen flame ionization detector and TCD dual detector) for online quantitative analysis to obtain real-time dimethylamine conversion, DMF selectivity and yield. The reaction conditions and the results at 120 h are shown in Table 3.
[0083] Table 3 Real-time reaction results of CO2 fixed bed catalytic conversion to DMF
[0084]
[0085] From the results in Table 3, it can be seen that the supported catalyst prepared in the present invention can achieve continuous conversion of CO2 and still has a high reaction activity after running for 120 hours.
[0086] Using the conventional impregnation method, catalysts with the same amount of active components as Example 4 (Pd-Ni / foamed-Al, Pd0.5Ni4.7wt%) and Example 5 (Ru-Ni / foamed-Al Ru2.5Ni4.7wt%) were prepared with foamed aluminum and alumina as carriers, namely Pd-Ni / foamed-Al-conventional, Ru-Ni / foamed-Al-conventional, Pd-Ni / Al2O3, and Ru-Ni / Al2O3, respectively. The performances were compared and the results are shown in Table 4.
[0087] Table 4 Comparison of performance of different catalysts
[0088]
[0089] From the results in Table 4, it can be seen that the metal-based foam material used as the carrier in the present invention and the metal-based foam-supported material prepared by the combustion method has better catalytic performance than the material obtained by the conventional impregnation method.
[0090] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A metal-based foam-supported material is used as a catalyst in the catalytic reaction of CO2, H2 and dimethylamine to prepare N,N-dimethylformamide, characterized in that: The metal-based foam-supported material comprises a metal-based foam carrier and a metal oxide supported on the metal-based foam carrier; the metal element in the metal oxide is one or more of Pd, Ru, Cu, Co and Ni.
2. The use according to claim 1, characterized in that: The metal-based foam carrier includes foamed aluminum, foamed copper or foamed nickel.
3. The use according to claim 1, characterized in that: The mass of the metal element in the metal oxide is 0.1-10% of the mass of the metal-based foam-supported material.
4. The use according to claim 1, characterized in that: The preparation method of the metal-based foam supported material comprises the following steps: Dissolving a metal oxide precursor and a combustion agent in water to obtain an impregnation solution; the combustion agent is urea, citric acid, glycine or ethylene glycol; Impregnating the metal-based foam carrier into the impregnation solution, and then calcining the obtained impregnation system to obtain the metal-based foam supported material; The metal oxide precursor is a soluble salt of a metal element; the metal element is one or more of Pd, Ru, Cu, Co and Ni.
5. The use according to claim 4, characterized in that: The molar ratio of the metal oxide precursor to the combustion agent is 1:0.8-3.
6. The use according to claim 4, characterized in that: The total mass concentration of the metal oxide precursor and the combustion agent in the impregnation solution is not less than 1.5%.
7. The use according to claim 4, characterized in that: The calcination is carried out in an air atmosphere; the calcination temperature is 500-800° C., and the heat preservation time is 5-10 minutes.
8. The use according to claim 4, characterized in that: The immersion time is 2 to 6 hours.
9. The use according to claim 1, characterized in that: The molar ratio of dimethylamine to CO2 is 1:1-10; the pressure of the reaction is 4-10 MPa, wherein the molar ratio of CO2 to H2 is 1:1-1.5; and the temperature of the reaction is 140-200°C.