A packaging film and its preparation method and application
By using POE matrix resin in the packaging film of photovoltaic modules, combining ultraviolet luminescent agents and fluorescent luminescent agents, combined with inorganic doped nano rare earth luminescent materials, the module's response ability to 280-380nm ultraviolet light is improved, and the photovoltaic module is solved The problems of photoconversion power generation efficiency and resistance to ultraviolet aging have achieved more efficient photoelectric conversion and ultraviolet resistance.
Patent Information
- Application Number
- CN202111521612.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-12-13
AI Technical Summary
The existing photovoltaic module packaging film has a low response to ultraviolet light of 280-380nm, resulting in low photoconversion power generation efficiency and insufficient UV aging resistance.
The packaging film is prepared by blending extrusion, casting, cooling, slitting and winding processes using POE matrix resin with a specific proportion of ultraviolet luminescent agent and fluorescent luminescent agent. The packaging film is prepared by using inorganic doped nano-rare earth luminescent materials as ultraviolet light. Transforming agent to improve the film's response ability to ultraviolet light.
It significantly improves the photoelectric conversion efficiency of photovoltaic modules, can effectively capture and store light energy at ultraviolet wavelengths, release it at night, extends the service life of the module, reduces yellowing caused by ultraviolet aging, and improves UV resistance.
Smart Images

Figure BDA0003407697950000021 
Figure BDA0003407697950000091 
Figure BDA0003407697950000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photovoltaic modules, and in particular to a packaging adhesive film and a preparation method and application thereof. Background Art
[0002] Double-sided double-glass modules are important photovoltaic modules. Double-sided double-glass photovoltaic modules are divided into five layers, from top to bottom: glass, upper encapsulation film, battery cells, lower encapsulation film, and glass. The incident light passes through the upper glass and upper encapsulation film to enter the battery cells, thereby producing a photovoltaic effect.
[0003] For photovoltaic modules, the choice of encapsulation film is crucial. As an encapsulation material, ethylene-vinyl acetate copolymer (EVA) has poor weather resistance. Long-term exposure to ultraviolet rays and water vapor can easily lead to degradation and yellowing, which reduces the conversion efficiency of solar cells. On the other hand, EVA film has poor resistance to PID attenuation. Under the conditions of -1500V and 192h, the power attenuation on the back side reaches between 20-40%, and the power attenuation on the front side also exceeds 5%. Therefore, double-sided double-glass photovoltaic modules are now generally encapsulated with POE film.
[0004] CN110628335A discloses an energy storage type POE photovoltaic encapsulation film and a preparation method thereof. The raw materials of the disclosed encapsulation film include: POE matrix resin, peroxide crosslinking agent, crosslinking auxiliary agent, silane coupling agent, and luminescent agent, and the luminescent agent is a phosphorescent luminescent agent. In the disclosed POE encapsulation film raw material system, a specific amount ratio of phosphorescent luminescent agent is introduced, and a one-time mixing and melt casting molding process step is adopted, so that the POE film prepared by the disclosed method can convert part of the light energy into chemical energy storage while effectively ensuring the main comprehensive performance indicators, thereby helping the photovoltaic module to generate electricity autonomously at night, overcoming the problem of intermittent power generation of conventional photovoltaic modules at night.
[0005] CN111518487A discloses a POE film for photovoltaic double-glass module encapsulation with a special anti-PID and a preparation method thereof. The POE film comprises the following raw materials in parts by weight: 1-30 parts of POE grafted modified resin, 90-95 parts of first POE resin, 0.01-0.5 parts of ultraviolet absorber, 0.1-0.5 parts of PID regulator, 0.01-0.5 parts of light stabilizer, 0.5-5 parts of cross-linking aid, 0.1-0.5 parts of coupling agent, 0.01-0.5 parts of antioxidant and 0.5-5 parts of cross-linking agent. The disclosed POE film has better anti-PID ability and anti-aging effect than the film currently used in the industry, and can ensure that the power attenuation of PID after 192 hours is controlled within 3.0%.
[0006] However, the current packaging film has a low response to ultraviolet light of 280-380nm, and the efficiency of light conversion to power generation is not high.
[0007] In summary, it is crucial to develop an encapsulation film with high UV light response and high light conversion efficiency for use in photovoltaic modules. Summary of the invention
[0008] In view of the deficiencies in the prior art, the object of the present invention is to provide an encapsulation adhesive film and a preparation method and application thereof. The encapsulation adhesive film has a high ultraviolet light response and is used in photovoltaic modules with high light conversion power generation efficiency.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a packaging film, wherein the packaging film comprises the following components in parts by weight:
[0011]
[0012] In the present invention, the encapsulation film uses POE as a matrix resin, and a UV luminescent agent and a fluorescent luminescent agent in a specific ratio cooperate with each other, wherein the UV luminescent agent can reduce the aging effect of ultraviolet rays on the POE film, improve the solar light conversion efficiency and do not affect the appearance of the component; the role of the fluorescent luminescent agent is to simultaneously capture and store part of the ultraviolet wavelength light energy, release it at night and continuously generate electricity; if the weight fraction of the UV luminescent agent is too high, it cannot be evenly dispersed and affects the light transmittance of the film; if the weight fraction of the UV luminescent agent is too low, it cannot induce sufficient light response; if the weight fraction of the fluorescent luminescent agent is too high, it affects the long-term aging resistance of the material; if the weight fraction of the fluorescent luminescent agent is too low, the released light energy is too low and the battery cannot respond.
[0013] In the present invention, the weight parts of the POE is 100 parts.
[0014] The weight portion of the ultraviolet light conversion agent is 0.1-0.6 parts, for example, 0.15 parts, 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts, 0.5 parts, 0.55 parts, etc.
[0015] The weight proportion of the fluorescent luminescent agent is 0.1-1.5 parts, for example, 0.2 parts, 0.3 parts, 0.4 parts, 0.6 parts, 0.8 parts, 1.0 parts, 1.2 parts, 1.4 parts, etc.
[0016] The weight proportion of the other auxiliary agents is 0.05-2.5 parts, for example, 0.1 parts, 0.2 parts, 0.4 parts, 0.6 parts, 0.8 parts, 1.0 parts, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts, 2.0 parts, 2.2 parts, 2.4 parts, etc.
[0017] Preferably, the ultraviolet light conversion agent comprises an inorganic doped nano rare earth luminescent material.
[0018] The reason why the ultraviolet light conversion agent of the present invention is preferably an inorganic doped nano rare earth luminescent material is that such luminescent material is an inorganic component, has excellent weather resistance and ultra-long light response life; and also has excellent properties such as narrow spectral line width and tunable fluorescence emission wavelength.
[0019] Preferably, the ultraviolet light conversion agent includes a nano-inorganic salt doped with any one of europium, erbium, lanthanum, actinium or samarium, or a combination of at least two of them, wherein typical but non-limiting combinations include: a nano-inorganic salt doped with a combination of europium and erbium, a nano-inorganic salt doped with a combination of lanthanum, actinium and samarium, a nano-inorganic salt doped with a combination of erbium, lanthanum, actinium and samarium, etc.
[0020] Preferably, the nano inorganic salt comprises any one of nano phosphate, nano silicate or nano vanadate or a combination of at least two thereof, wherein typical but non-limiting combinations include: a combination of nano phosphate and nano silicate, a combination of nano silicate and nano vanadate, a combination of nano phosphate, nano silicate and nano vanadate, etc.
[0021] Preferably, the fluorescent luminescent agent includes nano calcium halophosphate phosphor or rare earth phosphor.
[0022] Preferably, the other auxiliary agents include any one of a primary cross-linking agent, an auxiliary cross-linking agent, a light stabilizer, a coupling agent or an antioxidant, or a combination of at least two thereof.
[0023] Preferably, the primary cross-linking agent comprises tert-amyl peroxy (2-ethylhexyl) carbonate and / or tert-butyl peroxy (2-ethylhexyl) carbonate.
[0024] Preferably, the auxiliary cross-linking agent includes triallyl isocyanurate and / or trimethylolpropane trimethacrylate.
[0025] Preferably, the light stabilizer comprises di(2,2,6,6-tetramethyl-4-piperidinyl)sebacate (light stabilizer 770) and / or poly[[6-[(1,1,3,3-tetramethylbutyl)amine]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imine]-1,6-dihexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imine]]] (light stabilizer 944).
[0026] Preferably, the coupling agent includes any one of vinyl-tri(2-methoxyethoxy)silane, vinyl triethoxysilane, vinyl trimethoxysilane or isocyanate propylethoxysilane, or a combination of at least two thereof, wherein typical but non-limiting combinations include: a combination of vinyl-tri(2-methoxyethoxy)silane and vinyl triethoxysilane, a combination of vinyl triethoxysilane, vinyl trimethoxysilane and isocyanate propylethoxysilane, a combination of vinyl-tri(2-methoxyethoxy)silane, vinyl triethoxysilane, vinyl trimethoxysilane and isocyanate propylethoxysilane, and the like.
[0027] Preferably, the antioxidant comprises any one of hindered phenol antioxidants, hindered amine antioxidants or phosphate antioxidants, or a combination of at least two thereof, wherein typical but non-limiting combinations include: a combination of hindered phenol antioxidants and hindered amine antioxidants, a combination of hindered amine antioxidants and phosphate antioxidants, a combination of hindered phenol antioxidants, hindered amine antioxidants and phosphate antioxidants, etc.
[0028] Preferably, the weight portion of the main cross-linking agent is 0.4-0.7 parts, such as 0.45 parts, 0.5 parts, 0.55 parts, 0.6 parts, 0.65 parts, etc.
[0029] Preferably, the weight portion of the auxiliary cross-linking agent is 0.2-0.9 parts, for example, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, etc.
[0030] Preferably, the weight portion of the light stabilizer is 0.1-0.3 parts, for example, 0.12 parts, 0.14 parts, 0.16 parts, 0.18 parts, 0.2 parts, 0.22 parts, 0.24 parts, 0.26 parts, 0.28 parts, etc.
[0031] Preferably, the weight portion of the coupling agent is 0.1-0.3 parts, for example, 0.12 parts, 0.14 parts, 0.16 parts, 0.18 parts, 0.2 parts, 0.22 parts, 0.24 parts, 0.26 parts, 0.28 parts, etc.
[0032] Preferably, the weight portion of the antioxidant is 0.05-0.3 parts, for example, 0.12 parts, 0.14 parts, 0.16 parts, 0.18 parts, 0.2 parts, 0.22 parts, 0.24 parts, 0.26 parts, 0.28 parts, etc.
[0033] In a second aspect, the present invention provides a method for preparing the encapsulation film according to the first aspect, the preparation method comprising the following steps:
[0034] The packaging film is obtained by mixing POE, ultraviolet light conversion agent, fluorescent luminescent agent and other auxiliary agents according to the formula amount and then processing.
[0035] Preferably, the processing methods include blending extrusion, casting, cooling, slitting and winding in sequence.
[0036] Preferably, the temperature of the co-extrusion is 85-95°C, for example, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, etc.
[0037] As a preferred technical solution, the preparation method comprises the following steps:
[0038] POE, ultraviolet light conversion agent, fluorescent luminescent agent and other auxiliary agents are mixed according to the formula amount, and then extruded at 85-95° C. The extrudate is subjected to the processes of casting, cooling, slitting and winding to obtain the packaging film.
[0039] In a third aspect, the present invention provides a double-sided double-glass component, wherein the double-sided double-glass component comprises the packaging film described in the first aspect.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] (1) The photoelectric response efficiency of conventional encapsulation films to the ultraviolet wavelength of 280-380nm is only 70%. The encapsulation film of the present invention can convert the light energy of ultraviolet wavelength into visible light of 400-800nm wavelength, and at the same time, the fluorescent agent can capture and store part of the light energy of ultraviolet wavelength, release it at night and continuously generate electricity.
[0042] (2) The preparation process of the encapsulation film of the present invention is simple, and the addition of the ultraviolet light conversion agent has no significant effect on the basic properties of the POE film, while effectively improving the photoelectric conversion efficiency of the component.
[0043] (3) The encapsulation film of the present invention has excellent anti-ultraviolet performance. Compared with conventional encapsulation films, the light-converting POE film can fully utilize ultraviolet light with a wavelength of 280-380nm, greatly reducing the yellowing of photovoltaic modules due to ultraviolet aging during use.
[0044] (4) The packaging film of the present invention has a peel strength of 187.5-191.2 N / cm, a transmittance of 91.7%-92.1% before UV aging, a transmittance of 90.10%-91.20% after UV aging, a power of more than 458 W, and a CTM value of more than 101.5%. DETAILED DESCRIPTION
[0045] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0046] Example 1
[0047] The present embodiment provides a packaging film, which is composed of the following components in parts by weight: 100 parts of POE particles (purchased from Dow Chemical, brand 8660), 0.7 parts of main cross-linking agent tert-amyl peroxy (2-ethylhexyl) carbonate, 0.7 parts of auxiliary cross-linking agent triallyl isocyanurate, 0.2 parts of coupling agent γ-(methacryloyloxy)propyltrimethoxysilane, 0.7 parts of light stabilizer 770, 0.2 parts of antioxidant KK6001, 0.2 parts of europium-doped nano sodium tetraborate and 0.3 parts of nano calcium halophosphate phosphor.
[0048] The method for preparing the packaging film comprises the following steps:
[0049] POE particles, ultraviolet light conversion agent, fluorescent luminescent agent, main cross-linking agent, auxiliary cross-linking agent, light stabilizer, coupling agent and antioxidant are mixed according to the formula amount, extruded at 90° C. The extrudate is subjected to the steps of casting, cooling, slitting and winding to obtain the encapsulating film.
[0050] Example 2
[0051] The present embodiment provides a packaging film, which is composed of the following components in parts by weight: 100 parts of POE particles (purchased from Dow Chemical, brand 8669), 0.7 parts of main cross-linking agent peroxy (2-ethylhexyl) carbonate tert-amyl, 0.6 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of coupling agent γ-(methacryloyloxy)propyltrimethoxysilane, 0.2 parts of light stabilizer 770, 0.2 parts of antioxidant KK6001, 0.4 parts of europium-doped nano sodium tetraborate and 0.3 parts of nano calcium halophosphate phosphor.
[0052] The method for preparing the packaging film comprises the following steps:
[0053] POE particles, ultraviolet light conversion agent, fluorescent luminescent agent, main cross-linking agent, auxiliary cross-linking agent, light stabilizer, coupling agent and antioxidant are mixed according to the formula amount, extruded at 90° C. The extrudate is subjected to the steps of casting, cooling, slitting and winding to obtain the encapsulating film.
[0054] Example 3
[0055] The present embodiment provides a packaging film, which is composed of the following components in parts by weight: 100 parts of POE particles (purchased from Dow Chemical, brand 8660), 0.6 parts of main cross-linking agent peroxy (2-ethylhexyl) carbonate tert-amyl, 0.6 parts of auxiliary cross-linking agent trimethylolpropane trimethacrylate, 0.3 parts of coupling agent γ-(methacryloyloxy)propyltrimethoxysilane, 0.2 parts of light stabilizer 770, 0.2 parts of antioxidant KK6001, 0.6 parts of europium-doped nano sodium tetraborate and 0.3 parts of nano calcium halophosphate phosphor.
[0056] The method for preparing the packaging film comprises the following steps:
[0057] POE particles, ultraviolet light conversion agent, fluorescent luminescent agent, main cross-linking agent, auxiliary cross-linking agent, light stabilizer, coupling agent and antioxidant are mixed according to the formula amount, extruded at 90° C. The extrudate is subjected to the steps of casting, cooling, slitting and winding to obtain the encapsulating film.
[0058] Example 4
[0059] The difference between this embodiment and embodiment 1 is that the weight portion of the ultraviolet light conversion agent is 0.6 parts, and the rest is the same as embodiment 1.
[0060] Embodiment 5-6
[0061] The difference between Example 5-6 and Example 1 is that the weight proportions of the fluorescent luminescent agent are 0.1 parts (Example 5) and 1.5 parts (Example 6), respectively, and the rest are the same as Example 1.
[0062] Comparative Example 1
[0063] The difference between this comparative example and Example 1 is that the ultraviolet light conversion agent and the fluorescent luminescent agent are not included, and the rest are the same as Example 1.
[0064] Comparative Example 2
[0065] The difference between this comparative example and Example 2 is that the ultraviolet light conversion agent and the fluorescent luminescent agent are not included, and the rest are the same as Example 2.
[0066] Comparative Example 3
[0067] The difference between this comparative example and Example 3 is that the ultraviolet light conversion agent and the fluorescent luminescent agent are not included, and the rest are the same as Example 3.
[0068] Comparative Examples 4-5
[0069] The difference between Comparative Examples 4-5 and Example 1 is that the weight portions of the ultraviolet light conversion agent are 0.05 parts (Comparative Example 4) and 0.7 parts (Comparative Example 5), respectively, and the rest are the same as Example 1.
[0070] Comparative Examples 6-7
[0071] The difference between Comparative Examples 6-7 and Example 1 is that the weight proportions of the fluorescent luminescent agent are 0.05 parts (Example 6) and 1.6 parts (Example 7), respectively, and the rest are the same as Example 1.
[0072] Comparative Example 8
[0073] The difference between this comparative example and Example 1 is that the fluorescent luminescent agent is replaced by an ultraviolet luminescent agent of equal mass, and the rest is the same as Example 1.
[0074] Performance Testing
[0075] The encapsulation films described in Examples 1-6 and Comparative Examples 1-8 were tested as follows:
[0076] (1) Peel strength: Laminate the encapsulation film and glass and test the peel strength;
[0077] (2) UV test (UV200kwh / m 2 ): Observe the appearance and test the light transmittance;
[0078] (3) QE response curve and power: After laminating the encapsulation film and glass, expose them to sunlight and test the QE response curve and power;
[0079] CTM value: The CTM value indicates the degree of component power loss. The higher the CTM value, the smaller the degree of component power loss.
[0080] The peel strength test is carried out in accordance with GB / T 2790-1995, and the transmittance test is carried out in accordance with ISO9050.
[0081] Other test execution standards are IEC61215 and IEC61730.
[0082] The test results are summarized in Table 1.
[0083] Table 1
[0084]
[0085]
[0086] Analysis of the data in Table 1 shows that the peel strength of the packaging film of the present invention is between 187.5-191.2 N / cm, the transmittance before UV aging is between 91.7%-92.1%, the transmittance after UV aging is between 90.10%-91.20%, the power is above 458 W, and the CTM value is above 101.5%. The packaging film of the present invention has excellent UV resistance and can make full use of UV light with a wavelength of 280-380 nm, which greatly reduces the yellowing of photovoltaic modules due to UV aging during use and can also improve the photoelectric conversion efficiency of the modules.
[0087] Analysis of Comparative Example 1 and Example 1 shows that the performance of Comparative Example 1 is not as good as that of Example 1, wherein the addition of the UV conversion agent has no significant effect on the basic properties of the peel strength and transmittance of the encapsulation film. After UV aging, the transmittance of the encapsulation film of the present invention decreases more significantly, and the QE response efficiency, power and CTM value are all maintained at a high level, proving that the encapsulation film of the present invention has better performance than the conventional encapsulation film without the addition of UV conversion agent and fluorescent luminescent agent.
[0088] The comparative analysis between Comparative Example 2 and Example 2 is similar to the comparative analysis between Comparative Example 3 and Example 3.
[0089] Analysis of Comparative Example 8 and Example 1 shows that the performance of Comparative Example 8 is not as good as that of Example 1, proving that the performance of the encapsulation film formed by using only the ultraviolet light conversion agent without the fluorescent luminescent agent is poor.
[0090] From the analysis of comparative examples 4-5 and embodiments 1 and 4, and the analysis of comparative examples 6-7 and embodiments 5-6, it can be seen that the performance of comparative examples 4-5 is not as good as embodiments 1 and 4, and the performance of comparative examples 6-7 is not as good as embodiments 5-6, which proves that the ultraviolet light conversion agent and the fluorescent light conversion agent are used in combination in a specific proportion, and the synergistic effect forms a packaging film with better performance. If the weight fraction of the ultraviolet light conversion agent is outside the range of 0.1-0.6 parts, or the weight fraction of the fluorescent light conversion agent is outside the range of 0.1-1.5 parts, the performance of the formed packaging film is poor.
[0091] The present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A packaging film, characterized in that: The encapsulation film is composed of the following components in parts by weight: POE 100 copies Europium doped nano sodium tetraborate 0.1-0.6 parts Nano calcium halophosphate phosphor 0.1-1.5 parts Main cross-linking agent 0.4-0.7 parts Cross-linking agent 0.2-0.9 parts Light stabilizer 0.1-0.3 parts Coupling agent 0.1-0.3 parts Antioxidant 0.05-0.3 parts.
2. The packaging film according to claim 1, characterized in that: The primary cross-linking agent includes tert-amyl peroxy (2-ethylhexyl) carbonate and / or tert-butyl peroxy (2-ethylhexyl) carbonate.
3. The packaging film according to claim 1, characterized in that: The auxiliary cross-linking agent includes triallyl isocyanurate and / or trimethylolpropane trimethacrylate.
4. The packaging film according to claim 1, characterized in that: The light stabilizer includes di(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and / or poly[[6-[(1,1,3,3-tetramethylbutyl)amine]-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidinyl)imine]-1,6-dihexanediyl[(2,2,6,6-tetramethyl-4-piperidinyl)imine]].
5. The packaging film according to claim 1, characterized in that: The coupling agent includes any one of vinyl-tri(2-methoxyethoxy)silane, vinyl triethoxysilane, vinyl trimethoxysilane or isocyanate propylethoxysilane or a combination of at least two thereof.
6. The packaging film according to claim 1, characterized in that: The antioxidant includes any one of a hindered phenol antioxidant, a hindered amine antioxidant or a phosphate antioxidant, or a combination of at least two of them.
7. A method for preparing the encapsulation film according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: The encapsulation film is obtained by mixing POE, europium-doped nano sodium tetraborate, nano calcium halophosphate fluorescent powder, a main cross-linking agent, an auxiliary cross-linking agent, a light stabilizer, a coupling agent and an antioxidant according to a formula amount and then processing.
8. The preparation method according to claim 7, characterized in that: The processing methods include blending extrusion, casting, cooling, slitting and winding in sequence.
9. The preparation method according to claim 8, characterized in that: The temperature of the blending extrusion is 85-95°C.
10. The preparation method according to claim 7, characterized in that: The preparation method comprises the following steps: POE, europium-doped nano sodium tetraborate, nano calcium halophosphate phosphor, main crosslinking agent, auxiliary crosslinking agent, light stabilizer, coupling agent and antioxidant are mixed according to the formula, extruded at 85-95° C., and the extrudate is subjected to the steps of casting, cooling, slitting and winding to obtain the encapsulation film.
11. A double-sided double-glass component, characterized in that: The double-sided double-glass component comprises the packaging film according to any one of claims 1-6.