A catalyst for catalyzing methane to olefins and its preparation method and application
By embedding specific metal elements into the catalyst to form a stable structure catalyst, the problems of low selectivity of methane-based olefin ethylene and poor catalyst stability in the prior art are solved, and efficient ethylene selectivity and catalyst life under low temperature and normal pressure are achieved. extend.
Patent Information
- Application Number
- CN202111567206.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-12-20
AI Technical Summary
The prior art cannot effectively and stably improve the ethylene selectivity of methane-formed olefins, and the catalyst has problems such as particles prone to agglomeration and poor dispersion during long-term operation.
Using a catalyst with support TiO2, Al2O3 or SiO2, the Group VIII metal elements and Ag/Cu elements are embedded by atomic deposition method to form active metal components A and B with dispersed and continuous phases to control the total content and ratio of active metals. , form a stable structure to improve the activity and life of the catalyst.
During the plasma conversion of methane to olefins, the directional conversion of methane under low temperature and normal pressure is achieved, which significantly improves the selectivity of ethylene and extends the life of the catalyst.
Smart Images

Figure BDA0003422271190000161 
Figure BDA0003422271190000162
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalysts, specifically to a catalyst for plasma conversion of methane to olefins, its preparation method, and its application. Background Art
[0002] Ethylene, as one of the most important basic raw materials in the petrochemical industry, mainly originates from petroleum hydrocarbon cracking technology. However, due to significant fluctuations in oil prices, the ethylene market is heavily dependent on oil prices. Currently, my country is focusing on developing non-petroleum-based ethylene production processes, among which the coal-to-methanol-to-low-carbon-olefins process is well-developed. However, coal chemical processes consume large amounts of water and energy during the coal gasification stage, while most coal-rich areas are water-scarce, severely limiting the development of coal-to-olefins. With the development of combustible ice and shale gas, natural gas reserves are abundant, and natural gas conversion and utilization technologies have become a research hotspot. Developing processes for converting natural gas into ethylene as a national energy strategic reserve has become a new direction for technological development.
[0003] The process of producing ethylene from natural gas mainly involves anaerobic coupling and aerobic coupling. Aerobic coupling, due to the risk of combustion and explosion when flammable gas is mixed with an oxidizer and the demanding operating conditions, has not yet been industrialized. Anaerobic coupling utilizes natural gas to produce hydrogen and high-value-added olefins. In its traditional process, methane is converted through adsorption-activated coupling on the catalyst surface under high temperature and pressure conditions. However, anaerobic coupling produces numerous byproducts and cannot be directionally converted into ethylene.
[0004] Plasma conversion of natural gas involves activating methane through electron collisions under an electric field, followed by free radical collision coupling to form products. This plasma-based methane conversion can be carried out at ambient temperature and pressure, with relatively mild operating conditions and high selectivity for specific products, primarily acetylene.
[0005] CN109503310A discloses a process for producing high-concentration acetylene and hydrogen from natural gas. The process employs a plasma pyrolysis reactor, and after high-temperature pyrolysis and rapid cooling, carbon black, acetylene, and hydrogen are separated through a series of measures.
[0006] CN105451874A discloses a reactor for producing ethylene from methane, comprising a plasma source and a catalyst including a mesoporous support material. The methane feed passes through the plasma source and catalyst to obtain one or more downstream products of ethylene, hydrogen, and carbon. The catalyst provided by this prior art uses an impregnation method to add electronic promoters, improving the electronic environment around the active metal Pd and significantly enhancing the catalyst activity. However, the catalyst provided by this prior art suffers from the drawback of easy particle agglomeration and poor dispersion during the reaction, which is detrimental to long-term catalyst operation. Summary of the Invention
[0007] The purpose of this invention is to overcome the shortcomings of existing technologies that cannot effectively and stably improve the ethylene selectivity of methane-to-olefins production.
[0008] To achieve the above objectives, a first aspect of the present invention provides a catalyst for catalytic production of olefins from methane, the catalyst comprising a support and an active metal component supported on the support, the support being selected from at least one of TiO2, Al2O3, and SiO2, the active metal component comprising active metal component A and active metal component B, the active metal component A being embedded in the active metal component B, which exists in the form of a continuous phase, the active metal component A containing at least one of Group VIII metal elements, and the active metal component B containing Ag and / or Cu elements; based on the total weight of the catalyst, the content of the support is 98.9-99.89% by weight, the total content of the active metal component (calculated as oxides) is 0.11-1.1% by weight, and the weight ratio of the contents of active metal component A and active metal component B (calculated as oxides) is 1:1-100.
[0009] The second aspect of the present invention provides the application of the catalyst described in the first aspect in plasma conversion of methane to olefins.
[0010] A third aspect of the present invention provides a method for preparing the catalyst described in the first aspect, the method comprising:
[0011] (1) A metal source I containing at least one of the group VIII metal elements is deposited on a support by atomic deposition to obtain intermediate I. The intermediate I is then subjected to a first contact reaction with a modification solution to obtain intermediate II loaded with active metal component A. The modification solution is selected from at least one of aromatic carboxylic acids, saturated carboxylic acids, xylene, and propylbenzene.
[0012] (2) A metal source II containing Ag and / or Cu elements is cyclically deposited on intermediate II by atomic deposition to obtain intermediate III. Intermediate III is then reduced to obtain a catalyst.
[0013] The number of cycles in steps (1) and (2) is controlled such that the total content of the active metal component, based on the total weight of the catalyst and in terms of oxides, is 0.11-1.1% by weight, and the weight ratio of the active metal component A and the active metal component B, respectively, in terms of oxides, is 1:1-100.
[0014] The catalyst described in this invention has a stable structure, and the method of this invention can form an inert deposition layer around the active metal, extending the catalyst lifetime. Moreover, the prepared catalyst can adapt to the changes in the composition of the tail gas caused by the unstable discharge of the plasma process, and realize the directional conversion of methane to ethylene at low temperature and normal pressure, effectively and stably improving the selectivity of ethylene. Detailed Implementation
[0015] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0016] The following provides some exemplary explanations for certain functional groups of the present invention. Unless otherwise specified, the unlisted parts are explained with reference to the following exemplary explanations.
[0017] “C 1-5 "alkyl" refers to an alkyl group with a total number of carbon atoms of 1-5, including straight-chain alkyl and branched-chain alkyl. For example, it can be a straight-chain alkyl or branched-chain alkyl with a total number of carbon atoms of 1, 2, 3, 4, or 5, such as n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, etc.
[0018] As previously described, a first aspect of the present invention provides a catalyst for catalytic production of olefins from methane, the catalyst comprising a support and an active metal component supported on the support, the support being selected from at least one of TiO2, Al2O3, and SiO2, the active metal component comprising active metal component A and active metal component B, the active metal component A being embedded in the active metal component B, which exists in the form of a continuous phase, the active metal component A containing at least one of Group VIII metal elements, and the active metal component B containing Ag and / or Cu elements; based on the total weight of the catalyst, the content of the support is 98.9-99.89% by weight, the total content of the active metal component (calculated as oxides) is 0.11-1.1% by weight, and the weight ratio of the contents of active metal component A and active metal component B (calculated as oxides) is 1:1-100.
[0019] Preferably, the weight ratio of the active metal component A and the active metal component B, respectively calculated as oxides, is 1:10-100, more preferably 1:20-50.
[0020] Preferably, based on the total weight of the catalyst, the content of the support is 98.9-99.4% by weight, and the total content of the active metal component, calculated as oxides, is 0.6-1.1% by weight.
[0021] In a preferred embodiment, the active metal component A contains at least one metal element selected from Fe, Co, Ni, Pd, Ir, and Pt.
[0022] More preferably, the active metal component A contains at least one metal element selected from Pd, Ir, and Pt. The inventors have found that the catalyst in this preferred configuration exhibits higher ethylene selectivity.
[0023] According to a particularly preferred embodiment, the active metal component A contains Ag element, and the active metal component B contains Pd element; under this preferred embodiment, the catalyst has higher ethylene selectivity.
[0024] In a preferred embodiment, the catalyst has an average particle size of 3-5 mm.
[0025] More preferably, the catalyst has an average particle size of 3-3.5 mm.
[0026] As previously stated, a second aspect of the present invention provides the application of the catalyst described in the first aspect in plasma conversion of methane to olefins.
[0027] As previously described, a third aspect of the present invention provides a method for preparing the catalyst described in the first aspect, the method comprising:
[0028] (1) A metal source I containing at least one of the group VIII metal elements is deposited on a support by atomic deposition to obtain intermediate I. The intermediate I is then subjected to a first contact reaction with a modification solution to obtain intermediate II loaded with active metal component A. The modification solution is selected from at least one of aromatic carboxylic acids, saturated carboxylic acids, xylene, and propylbenzene.
[0029] (2) A metal source II containing Ag and / or Cu elements is cyclically deposited on intermediate II by atomic deposition to obtain intermediate III. Intermediate III is then reduced to obtain a catalyst.
[0030] The number of cycles in steps (1) and (2) is controlled such that the total content of the active metal component, based on the total weight of the catalyst and in terms of oxides, is 0.11-1.1% by weight, and the weight ratio of the active metal component A and the active metal component B, respectively, in terms of oxides, is 1:1-100.
[0031] The present invention does not impose any particular limitation on the time of each cycle. For example, the time of each cycle is 0.05-2 seconds.
[0032] In particular, the inventors have discovered that by controlling the number of cycles in steps (1) and (2) such that the total content of the active metal component, calculated as oxide, is 0.6-1.1% by weight based on the total weight of the catalyst, and the weight ratio of the active metal component A and the active metal component B, calculated as oxide, is 1:20-50, the resulting catalyst exhibits higher ethylene selectivity.
[0033] In a preferred embodiment, the metal source I is selected from at least one organic compound of at least one of the metal elements selected from Fe, Co, Ni, Pd, Ir, and Pt.
[0034] More preferably, the metal source I is selected from at least one of the organic compounds of palladium, organic compounds of iridium, and organic compounds of platinum.
[0035] Particularly preferably, the metal source I is selected from at least one of the following: palladium hexafluoroacetylacetonate (Pd(hfac)2), tri(acetylacetonate)palladium (Pd(acac)2), bis(1,5-cyclooctadiene)iridium chloride dimer ([Ir(cod)Cl]2), iridium acetylacetonate bis(2-benzothiazole-C2,N) iridium (Ir(btb)2(acac)), trimethyl(methylcyclopentadienyl)platinum (MeCpPtMe3), and (1,5-cyclooctadiene)dimethylplatinum (Pt(cod)(Me)2).
[0036] In a preferred embodiment, the metal source II is selected from at least one of the following: (triethylphosphine)pentanoyl silver (Ag(Piv)(PEt3)), (1,5-cyclooctadiene)hexafluoroacetylacetonate silver ((hfac)Ag(1,5-COD)), (triethylphosphine)(6,6,7,8,8,8-heptafluoro-2,2-dimethyl-3,5-octanoic acid) silver (Ag(fod)(PEt3)), trimethylphosphine (hexafluoroacetylacetonate) silver ((hfac)Ag(PMe3)), and copper acetylacetonate (Cu(acac)2).
[0037] According to a preferred embodiment, in steps (1) and (2), the number of cycles is independently greater than 0 and less than or equal to 600.
[0038] Preferably, in step (1), the number of cycles is 150-400.
[0039] Particularly preferably, in step (2), the number of cycles is 10-100.
[0040] According to another preferred embodiment, in steps (1) and (2), the conditions of the atomic deposition method are each independently satisfied at least as follows: temperature of 50-400℃, pressure of 0-200Pa, and time of 20-800s.
[0041] Preferably, in steps (1) and (2), the pulse frequencies of the metal source I and the metal source II are each independently 50-2000ms.
[0042] Preferably, in step (1), the conditions for the first contact reaction are at least: temperature of 50-400℃, pressure of 0-200Pa, and time of 20-800s.
[0043] Preferably, in step (1), the weight ratio of the modified solution to the metal source I is 1:1-2.
[0044] Preferably, the pulse frequency of the modified solution is 1-2 times that of the pulse frequency of the gold source I.
[0045] Preferably, the modified solution is selected from at least one of benzoic acid, phthalic acid, glacial acetic acid, xylene, and propylbenzene.
[0046] Preferably, in step (2), the reduction reaction is carried out in the presence of a reducing agent with the structural formula R1R2N-NR3R4, wherein R1, R2, R3, and R4 are each independently selected from H, C, and C. 1-5 Any one of the alkyl groups.
[0047] Preferably, the reducing agent is selected from at least one of anhydrous hydrazine, methylhydrazine, ethylhydrazine, propylhydrazine, and tert-butylhydrazine.
[0048] Preferably, in step (2), the pulse frequency of the reducing agent is 10-500ms.
[0049] In a preferred embodiment, in step (2), the conditions for the reduction reaction are at least: a temperature of 50-400°C and a pressure of 0-200Pa.
[0050] According to a particularly preferred embodiment, the temperature of each of the metal sources is independently 100-150°C prior to each of the depositions.
[0051] According to a particularly preferred embodiment, the temperature of the reducing agent is 30-70°C before the reduction reaction is carried out.
[0052] According to another particularly preferred embodiment, before applying intermediate I, it is first contacted with an inert gas for cleaning I; before applying intermediate III, it is first contacted with oxygen for cleaning II.
[0053] Preferably, the inert gas is selected from at least one of argon and helium.
[0054] Preferably, the cleaning time is 1-200s.
[0055] Preferably, the temperature of the second cleaning step is 400-550°C and the time is 60-300 seconds.
[0056] The terms "cleaning I" and "cleaning II" refer to the following: intermediate I is first cleaned by contacting with an inert gas before the first contact reaction is performed; intermediate III is first cleaned by contacting with oxygen before the reduction reaction is performed.
[0057] According to a preferred embodiment, the catalyst preparation process is carried out in an atomic deposition apparatus (e.g., an ALD deposition apparatus), which includes a metal source tank I, a metal source tank II, a reducing agent cylinder, a reaction chamber, a transport pipeline, and an ALD valve.
[0058] According to a particularly preferred embodiment, the process for preparing the catalyst includes at least the following steps:
[0059] (1) Liquid metal source I, liquid metal source II, reducing agent and carrier to be plated are respectively loaded into metal source tank I, metal source tank II, reducing agent cylinder and reaction chamber;
[0060] (2) Heat each metal source tank to 140-170℃, reducer cylinder to 30-70℃, reaction chamber to 50-400℃, transport pipeline and ALD valve to 180-200℃, and evacuate the reaction chamber and transport pipeline to a pressure of 10-200Pa.
[0061] (3) Open the ALD pulse valve of the metal source tank I for 50-2000ms to circulate the liquid metal source I into the reaction chamber, where it undergoes self-saturation adsorption with the carrier surface, reacts and deposits to obtain intermediate I. After the deposition is completed, inert gas is introduced into the reaction chamber to clean the unreacted metal source and the by-products generated by the reaction. The cleaning time is 1-200s.
[0062] (4) Intermediate I is reacted with the modified solution in a first contact reaction for 20-800 s to obtain intermediate II;
[0063] (5) Open the ALD pulse valve of the metal source tank II for 50-2000ms to circulate the liquid metal source II into the reaction chamber, where it undergoes self-saturation adsorption with the surface of intermediate II, reacts and deposits to obtain intermediate III. After the deposition is completed, oxygen is introduced into the reaction chamber and the temperature of the reaction chamber is raised to 400-550℃ to clean the unreacted modified solution and byproducts. The cleaning time is 60-300s.
[0064] (6) Open the ALD pulse valve of the reducing agent cylinder for 10-500ms to bring the reducing agent into the reaction chamber, where it undergoes chemical adsorption with intermediate III and a reduction reaction to generate a reduced metal state. After the reaction is complete, inert gas is introduced into the reaction chamber to clean the unreacted reducing agent and the by-products generated by the reaction. The cleaning time is 1-200s to obtain the catalyst sample.
[0065] (7) The catalyst sample is calcined in air and formed by a ball rolling machine in sequence to obtain the catalyst.
[0066] Preferably, the roasting temperature is 400-500℃ and the time is 3-6 hours.
[0067] It should be noted that the present invention does not impose any particular limitation on the preparation method of the substrate to be plated. Any method known in the art can be used for preparation. The following examples of the present invention provide a specific operation, which should not be construed as a limitation of the present invention by those skilled in the art.
[0068] The present invention will be described in detail below through examples. In the following examples, unless otherwise specified, all raw materials used are commercially available products.
[0069] Al2O3: Purchased from Aladdin Reagent, with an average particle size of 3 mm;
[0070] TiO2: Purchased from Aladdin Reagent, with an average particle size of 3 mm;
[0071] SiO2: Purchased from Aladdin Reagent, with an average particle size of 3 mm;
[0072] Palladium hexafluoroacetylacetone (Pd(hfac)2): purchased from Aladdin Reagents;
[0073] (Triethylphosphorus)Pentaylsilver (Ag(Piv)(PEt3)): purchased from Aladdin Reagents;
[0074] Bis(1,5-cyclooctadiene)iridium chloride dimer ([Ir(cod)Cl]2): purchased from Aladdin Reagents;
[0075] (1,5-Cyclooctadiene)dimethylplatinum (Pt(cod)(Me)2): purchased from Aladdin Reagents;
[0076] Copper acetylacetonate (Cu(acac)2): purchased from Aladdin Reagents;
[0077] Modified solution (benzoic acid): purchased from Aladdin Reagents;
[0078] Reducing agent (anhydrous hydrazine): purchased from Aladdin Reagents;
[0079] Plasma reactor: See patent document CN109289457A, specifically, the plasma reactor includes a blade sliding arc stabilization system and a reactor:
[0080] The blade sliding arc stabilization system includes a first DC power supply, a second DC power supply, an inductor coil, a diode, and an electromagnetic relay switch. The first DC power supply is connected in series with the inductor coil and the diode. The electromagnetic relay switch and the second DC power supply are connected in series. The two series branches are connected in parallel and then connected to the two electrodes of the reactor. The positive and negative terminals of the two DC power supplies are in the same direction and the negative terminal is grounded. The first DC power supply is a 1.5kV DC power supply, the second DC power supply is a 10kV DC power supply, and the inductor coil 6 is a 30mH inductor coil. The breakdown voltage is provided by the second DC power supply, and the power supply is maintained by the first DC power supply.
[0081] The reactor includes an outer casing, two electrodes, two flat magnets, and a nozzle. The electrodes are arc-shaped blade electrodes (20mm radius), arranged on the lower wall of the reactor and placed opposite each other. The outer casing is a straight quadrangular prism structure with a rectangular cross-section (made of quartz, 45mm*12mm*110mm, wall thickness 2mm). The two flat magnets are arranged parallel to each other on the outside of the outer casing. The nozzle (2mm diameter) is located on the lower wall of the reactor corresponding to the center of the two electrodes, injecting gas into the reactor. The nozzle outlet is 10mm away from the narrowest point of the two electrodes. The upper and lower walls of the reactor are made of high-temperature resistant insulating alumina ceramic. Graphite gaskets are placed between the upper and lower walls and the outer casing. The upper and lower walls are pressed together by screws and nuts to fix the outer casing.
[0082] The reaction processes in the following examples were all carried out in an ALD deposition apparatus (model Savannah G2 ALD).
[0083] Example 1
[0084] (1) Heat the metal source tank I containing liquid palladium metal source and the metal source tank II containing liquid silver metal source to 150°C respectively, heat the reducing agent cylinder containing reducing agent to 30°C, heat the reaction chamber to 80°C, heat the transport pipeline and ALD valve to 180°C, and evacuate the reaction chamber and transport pipeline to a pressure of 100Pa.
[0085] (2) Weigh 40g of Al2O3 and mix it with anhydrous ethanol (80ml). Disperse it by sonication for 3min to obtain a suspension. Use a dropper to take 2ml of the suspension and drop it onto a quartz plate. Spread it evenly and let it dry naturally before transferring it to the reaction chamber.
[0086] (3) Open the ALD pulse valve of metal source tank I for 100ms to bring the liquid palladium metal source (Pd(hfac)2) into the reaction chamber, where it undergoes self-saturation adsorption and reaction with the Al2O3 support surface, and 40 palladium metal sources are cyclically deposited to obtain intermediate I. After the deposition is completed, helium gas is introduced into the reaction chamber to clean the unreacted metal sources and the by-products generated by the reaction. The cleaning time is 100s.
[0087] (4) Intermediate I was contacted with the modified solution (xylene) for 40 s to obtain intermediate II;
[0088] (5) Open the ALD pulse valve of the metal source tank II for 100ms to bring the liquid silver metal source (Ag(Piv)(PEt3)) into the reaction chamber, where it undergoes self-saturation adsorption and reaction with the surface of intermediate II. Then, 200 silver metal sources are circulated and deposited to obtain intermediate III. After the deposition is completed, oxygen is introduced into the reaction chamber and the temperature of the reaction chamber is raised to 500℃ to clean the unreacted modified solution and by-products. The cleaning time is 60s.
[0089] (6) Open the ALD pulse valve of the reducing agent cylinder for 100ms to bring the anhydrous hydrazine reducing agent into the reaction chamber, where it undergoes chemical adsorption and reaction with intermediate III to generate a reduced metal state. After the reaction is complete, helium gas is introduced into the reaction chamber to clean the unreacted reducing agent and the by-products generated by the reaction. The cleaning time is 100s to obtain sample S1.
[0090] (7) Scrape sample S1 off the quartz plate, calcine it in an air atmosphere muffle furnace at 450℃ for 4 hours, and shape it by a ball rolling machine to obtain catalyst S1.
[0091] Example 2
[0092] The process flow of this embodiment is the same as that of Embodiment 1, except that:
[0093] Catalyst S2 was obtained by replacing the palladium metal source (Pd(hfac)2) with an equal weight of iridium metal source ([Ir(cod)Cl]2).
[0094] Example 3
[0095] The process flow of this embodiment is the same as that of Embodiment 1, except that:
[0096] Catalyst S3 was obtained by replacing the palladium metal source (Pd(hfac)2) with an equal weight of platinum metal source (Pt(cod)(Me)2).
[0097] Example 4
[0098] The process flow of this embodiment is the same as that of Embodiment 1, except that:
[0099] Catalyst S4 was obtained by replacing Al2O3 with an equal weight of TiO2.
[0100] Example 5
[0101] The process flow of this embodiment is the same as that of Embodiment 1, except that:
[0102] Catalyst S5 was obtained by replacing Al2O3 with an equal weight of SiO2.
[0103] Example 6
[0104] The process flow of this embodiment is the same as that of Embodiment 1, except that:
[0105] Catalyst S6 was obtained by replacing the silver metal source (Ag(Piv)(PEt3)) with an equal weight of copper metal source (Cu(acac)2).
[0106] Example 7
[0107] The process flow of this embodiment is the same as that of Embodiment 1, except that:
[0108] Catalyst S7 was obtained by replacing the silver source (Ag(Piv)(PEt3)) with an equal weight of copper source (Cu(acac)2) and the palladium source (Pd(hfac)2) with an equal weight of iridium source ([Ir(cod)Cl]2).
[0109] Example 8
[0110] The process flow of this embodiment is the same as that of Embodiment 1, except that:
[0111] Catalyst S8 was obtained by replacing the silver source (Ag(Piv)(PEt3)) with an equal weight of copper source (Cu(acac)2) and the palladium source (Pd(hfac)2) with an equal weight of platinum source (Pt(cod)(Me)2).
[0112] Example 9
[0113] The process flow of this embodiment is the same as that of Embodiment 1, except that:
[0114] The silver metal source was cycled and deposited 300 times to obtain catalyst S9.
[0115] Example 10
[0116] The process flow of this embodiment is the same as that of Embodiment 1, except that:
[0117] The palladium metal source was cycled and deposited 60 times to obtain catalyst S10.
[0118] Comparative Example 1
[0119] The comparative example has the same process flow as Example 1, except that:
[0120] A catalyst with only a single active metal component was obtained by cyclic deposition and reduction of only 200 silver metal sources (Ag(Piv)(PEt3)), specifically:
[0121] (1) Heat the metal source tank II containing liquid silver metal source to 150°C, heat the reducing agent cylinder containing reducing agent to 30°C, heat the reaction chamber to 80°C, heat the transport pipeline and ALD valve to 180°C, and evacuate the reaction chamber and transport pipeline to a pressure of 100Pa.
[0122] (2) Weigh 40g of Al2O3 and mix it with anhydrous ethanol (80ml). Disperse the mixture by sonication for 3min to obtain a suspension. Use a dropper to take 2ml of the suspension and drop it onto a quartz plate. Spread it evenly and let it dry naturally before transferring it to the reaction chamber.
[0123] (3) Open the ALD pulse valve of metal source tank II for 100ms to bring the liquid silver metal source (Ag(Piv)(PEt3)) into the reaction chamber, where it undergoes self-saturation adsorption and reaction with the Al2O3 support surface, and 200 silver metal sources are cyclically deposited to obtain intermediate I. After the deposition is completed, helium gas is introduced into the reaction chamber to clean the unreacted metal sources and the by-products generated by the reaction. The cleaning time is 100s.
[0124] (4) Open the ALD pulse valve of the reducing agent cylinder for 100ms to bring the anhydrous hydrazine reducing agent into the reaction chamber, where it undergoes chemical adsorption and reaction with intermediate I to generate a reduced metal state, thus obtaining intermediate II loaded with a silver metal layer. After the reaction is complete, helium gas is introduced into the reaction chamber to clean the unreacted reducing agent and the by-products generated by the reaction. The cleaning time is 100s, and sample D1 is obtained.
[0125] (5) Scrape sample D1 off the quartz plate, calcine it in an air atmosphere muffle furnace at 450℃ for 4 hours, and shape it by a ball rolling machine to obtain catalyst D1.
[0126] Comparative Example 2
[0127] The comparative example has the same process flow as Example 1, except that:
[0128] A catalyst with only a single active metal component was obtained by cyclic deposition and reduction of only 40 palladium metal sources (Ag(Piv)(PEt3)), specifically:
[0129] (1) Heat the metal source tank I containing liquid palladium metal source to 150°C, heat the reducing agent cylinder containing reducing agent to 30°C, heat the reaction chamber to 80°C, heat the transport pipeline and ALD valve to 180°C, and evacuate the reaction chamber and transport pipeline to a pressure of 100Pa.
[0130] (2) Weigh 40g of Al2O3 and mix it with anhydrous ethanol (80ml). Disperse the mixture by sonication for 3min to obtain a suspension. Use a dropper to take 2ml of the suspension and drop it onto a quartz plate. Spread it evenly and let it dry naturally before transferring it to the reaction chamber.
[0131] (3) Open the ALD pulse valve of metal source tank I for 100ms to bring the liquid palladium metal source (Pd(hfac)2) into the reaction chamber, where it undergoes self-saturation adsorption and reaction with the surface of intermediate II. Then, perform 40 palladium metal sources in a cycle to deposit intermediate III. After the deposition is completed, helium gas is introduced into the reaction chamber to clean the unreacted metal sources and the byproducts generated in the reaction. The cleaning time is 100s.
[0132] (4) Open the ALD pulse valve of the reducing agent cylinder for 100ms to bring the anhydrous hydrazine reducing agent into the reaction chamber, where it undergoes chemical adsorption and reaction with intermediate III to generate a reduced metal state. After the reaction is complete, helium gas is introduced into the reaction chamber to clean the unreacted reducing agent and the by-products generated by the reaction. The cleaning time is 100s to obtain sample D2.
[0133] (5) Scrape sample D2 off the quartz plate, calcine it in an air atmosphere muffle furnace at 450℃ for 4 hours, and shape it by a ball rolling machine to obtain catalyst D2.
[0134] Comparative Example 3
[0135] The process flow of this comparative example is the same as that of Comparative Example 2, except that:
[0136] Catalyst D3 was obtained by replacing the palladium metal source (Pd(hfac)2) with an equal weight of iridium metal source ([Ir(cod)Cl]2).
[0137] Comparative Example 4
[0138] The process flow of this comparative example is the same as that of Comparative Example 2, except that:
[0139] Catalyst D4 was obtained by replacing the palladium metal source (Pd(hfac)2) with an equal weight of platinum metal source (Pt(cod)(Me)2).
[0140] Comparative Example 5
[0141] The process flow of this comparative example is the same as that of Comparative Example 2, except that:
[0142] Catalyst D5 was obtained by replacing Al2O3 with an equal weight of TiO2.
[0143] Test Example 1
[0144] Each catalyst (40g) in the aforementioned example was placed in a plasma reactor for reaction: the inlet flow rate was 0.5L / min for methane, 1.5L / min for hydrogen, and the discharge power was 120W. The methane conversion rate and ethylene selectivity were calculated, and the corresponding process conditions and results are shown in Table 1.
[0145] The methane conversion rate is calculated using the following formula:
[0146] Methane conversion rate = (molecular amount of methane inlet - molecular amount of methane outlet) / molecular amount of methane inlet.
[0147] Ethylene selectivity is calculated using the following formula:
[0148] Ethylene selectivity = (Ethylene outlet molar amount) * 2 / (Methane import molar amount - Methane outlet molar amount).
[0149] (The molar amount of gas taken at the inlet or outlet per minute after the reaction has reached equilibrium is expressed as the amount of gas taken at the inlet or outlet.)
[0150] Test Example 2:
[0151] 40g of catalyst S1 was placed in a plasma reactor for catalyst stability evaluation: the inlet flow rate was 0.5L / min for methane, 1.5L / min for hydrogen, 1.5L / min for carbon monoxide, and the discharge power was 110W. The methane conversion rate and ethylene selectivity were recorded.
[0152] Evaluation results: Methane conversion rate remained at 30-40%, ethylene selectivity remained above 93%, and the duration of maintenance was 400 hours.
[0153] Table 1
[0154]
[0155]
[0156] Table 1 (continued)
[0157]
[0158] The evaluation results above and the results in Table 1 show that the method of the present invention effectively improves the catalyst lifetime, and the catalyst of the present invention effectively and stably improves the ethylene selectivity of methane to olefins, and has broad application prospects.
[0159] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.
Claims
1. A catalyst for catalyzing methane to olefins, It is characterized in that The catalyst contains a carrier and an active metal component supported on the carrier, and the carrier is selected from TiO 2 、Al 2 O 3 、SiO 2 At least one of the active metal components, the active metal component comprises an active metal component A and an active metal component B, the active metal component A is embedded in the active metal component B in the form of a continuous phase in the form of a dispersed phase, the active metal component A contains at least one of Pd, Ir, and Pt metal elements, and the active metal component B contains Ag element and / or Cu element; based on the total weight of the catalyst, the content of the carrier is 98.9-99.89% by weight, the total content of the active metal components calculated as oxides is 0.11-1.1% by weight, and the weight ratio of the active metal component A to the active metal component B calculated as oxides is 1:1-100; The catalyst is prepared by a method comprising the following steps: (1) using an atomic deposition method to cyclically deposit a metal source I containing at least one of Pd, Ir, and Pt metal elements on a carrier to obtain an intermediate I, and subjecting the intermediate I to a first contact reaction with a modified solution to obtain an intermediate II loaded with an active metal component A, wherein the modified solution is selected from at least one of aromatic carboxylic acid, saturated carboxylic acid, xylene, and propylbenzene; (2) using an atomic deposition method to cyclically deposit a metal source II containing an Ag element and / or a Cu element on the intermediate II to obtain an intermediate III, and subjecting the intermediate III to a reduction reaction to obtain a catalyst; The number of cycles in step (1) and step (2) is controlled so that the total content of the active metal component calculated as oxide is 0.11-1.1 wt % based on the total weight of the catalyst, and the weight ratio of the active metal component A to the active metal component B calculated as oxide is 1:1-100.
2. The catalyst according to claim 1, in, The weight ratio of the active metal component A to the active metal component B, calculated as oxides, is 1:10-100.
3. The catalyst according to claim 2, in, The weight ratio of the active metal component A to the active metal component B, calculated as oxides, is 1:20-50.
4. The catalyst according to any one of claims 1 to 3, in, Based on the total weight of the catalyst, the content of the carrier is 98.9-99.4 wt %, and the total content of the active metal components calculated as oxides is 0.6-1.1 wt %.
5. The catalyst according to any one of claims 1 to 3, in, The average particle size of the catalyst is 3-5 mm.
6. The catalyst according to any one of claims 1 to 3, in, The metal source I is selected from at least one of an organic compound of palladium, an organic compound of iridium and an organic compound of platinum.
7. The catalyst according to claim 6, in, The metal source I is selected from (Pd(hfac) 2 )、Pd(acac) 2 、[Ir(cod)Cl] 2 、Ir(btb) 2 (acac), MeCpPtMe 3 、Pt(cod)(Me) 2 At least one of .
8. The catalyst according to any one of claims 1 to 3, in, The metal source II is selected from Ag(Piv)(PEt 3 ), (hfac)Ag(1,5-COD), Ag(fod)(PEt 3 )、(hfac)Ag(PMe 3 )、Cu(acac) 2 At least one of .
9. The catalyst according to any one of claims 1 to 3, in, In step (1) and step (2), the number of cycles is independently greater than 0 and less than or equal to 600.
10. The catalyst according to claim 9, in, In step (1), the number of cycles is 150-400.
11. The catalyst according to claim 9, in, In step (2), the number of cycles is 10-100.
12. The catalyst according to any one of claims 1 to 3, in, In step (1) and step (2), the conditions of the atomic deposition method independently satisfy at least the following: temperature of 50-400° C., pressure of 0-200 Pa, and time of 20-800 s.
13. The catalyst according to any one of claims 1 to 3, in, In step (1) and step (2), the pulse frequencies of the metal source I and the metal source II are independently 50-2000 ms.
14. The catalyst according to any one of claims 1 to 3, in, In step (1), the conditions of the first contact reaction at least meet the following conditions: temperature of 50-400° C., pressure of 0-200 Pa, and time of 20-800 s.
15. The catalyst according to any one of claims 1 to 3, in, In step (2), the reduction reaction is carried out in the case of a compound having the structural formula R 1 R 2 N-NR 3 R 4 In the presence of a reducing agent, the R 1 , R 2 , R 3 , R 4 Each independently selected from H, C 1-5 Any one of the alkyl groups.
16. The catalyst according to claim 15, in, The reducing agent is selected from at least one of anhydrous hydrazine, methyl hydrazine, ethyl hydrazine, propyl hydrazine and tert-butyl hydrazine.
17. The catalyst according to claim 16, in, In step (2), the reduction reaction conditions at least meet the following conditions: temperature of 50-400° C. and pressure of 0-200 Pa.
18. The catalyst according to claim 17, in, In step (2), the pulse frequency of the reducing agent is 10-500 ms.
19. The catalyst according to any one of claims 1 to 3, in, Prior to each of the depositions, the temperature of each of the metal sources is independently 100-150°C.
20. The catalyst according to any one of claims 1 to 3, in, The method further comprises: before using the intermediate I, first contacting the intermediate I with an inert gas to clean the intermediate I I; before using the intermediate III, first contacting the intermediate III with oxygen to clean the intermediate III II.
21. The catalyst according to claim 20, in, The inert gas is selected from at least one of argon and helium.
22. The catalyst according to claim 20, in, The intermediate I is cleaned for a cleaning time of 1-200s.
23. The catalyst according to claim 20, in, The temperature of the cleaning II for cleaning the intermediate III is 400-550° C. and the time is 60-300 seconds.
24. Use of the catalyst according to any one of claims 1 to 23 in plasma conversion of methane to olefins.
Citation Information
Patent Citations
Reactor comprising a plasma source and a catalyst comprising a mesoporous support material for the preparation of ethene from methane
CN105451874A
Greenhouse gas conversion device and method utilizing magnetic field to strengthen blade gliding arc
CN109289457A
Technology for preparing high-concentration acetylene and hydrogen from natural gas
CN109503310A
Catalyst for preparing olefin by dehydrogenating low-carbon alkane and preparation method of catalyst
CN104148062A