A kind of anti-aging modified asphalt waterproofing membrane and preparation method thereof

By adding modified nano-zeolite and modified nano-montmorillonite to asphalt waterproof membranes, combined with SBS and light stabilizers, an elastic network structure is formed, solving the problem of easy aging of asphalt waterproof membranes and achieving significant improvement in anti-aging performance and enhanced stability.

CN116285762BActive Publication Date: 2024-11-12TIANJIN YUSHEN BUILDING WATERPROOF MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310339801.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-11-12
Estimated Expiration
2043-04-03

AI Technical Summary

Technical Problem

Existing asphalt waterproof membranes are prone to aging during long-term use, especially under conditions of sun exposure, rain, and thermal expansion and contraction, which leads to the failure of their waterproof function. The anti-aging performance of membranes with added nano-titanium dioxide is not outstanding.

Method used

Modified nano-zeolite and modified nano-montmorillonite are mixed with petroleum asphalt, combined with SBS, anti-aging agents and light stabilizers to form an elastic network structure. This structure adsorbs lightweight small molecules, enhances stability, and improves the anti-aging performance of waterproof membranes by improving compatibility and filling gaps.

Benefits of technology

It significantly improves the anti-aging properties and stability of asphalt waterproof membranes, extends their service life, and has a simple preparation method suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application relates to the field of waterproofing rolls, and specifically discloses an anti-aging modified asphalt waterproofing roll and a preparation method thereof. An anti-aging modified asphalt waterproofing roll comprises a polyester base fabric, a modified asphalt layer coated on the polyester base fabric, and a polyethylene film coated on the modified asphalt layer, wherein the modified asphalt layer comprises the following raw materials in parts by weight: 42‑48 parts of petroleum asphalt, 8‑10 parts of base oil, 6‑10 parts of SBS, 6‑10 parts of SBR, 3‑7 parts of terpene resin, 5‑8 parts of anti-aging agent, 3‑5 parts of light stabilizer, 5‑7 parts of modified nano zeolite, and 8‑12 parts of modified nano montmorillonite. The asphalt waterproofing roll of the present application has the characteristics of excellent anti-aging performance and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of waterproofing membranes, and more specifically, to an anti-aging modified asphalt waterproofing membrane and a preparation method thereof. Background Art

[0002] Waterproofing membrane is a rollable sheet-shaped waterproofing material. It is one of the important varieties of waterproofing materials for construction projects. Waterproofing membrane is mainly used in building walls, roofs, tunnels, roads, landfills, etc. It is a kind of flexible building material product that can be rolled into a roll to resist the leakage of rainwater and groundwater from the outside. As a leak-free connection between the engineering foundation and the building, it is the first barrier to waterproofing the entire project and plays a vital role in the entire project.

[0003] Asphalt waterproofing membranes are exposed to the sun and rain for a long time during use, and are also subject to environmental effects such as heat and oxygen, and are very easy to age. In addition, when used in the severely cold northern regions, they will be subjected to the phenomenon of thermal expansion and contraction caused by the alternating temperature difference between day and night, which will cause the membrane to crack and other damage. Taking the building roof waterproofing membrane as an example, the damage of the membrane will directly lead to building leakage, thus affecting people's normal production and life. Therefore, the anti-aging performance of asphalt waterproofing membranes must be particularly outstanding to ensure the normal performance of their waterproofing functions. However, the asphalt waterproofing membranes currently on the market generally achieve the purpose of anti-aging by adding nano-titanium dioxide to resist ultraviolet rays. The anti-aging performance of such waterproofing membranes is not outstanding enough, which eventually causes damage to the waterproofing membranes and affects their normal use. Summary of the invention

[0004] In order to improve the anti-aging performance of asphalt waterproofing membranes, the present application provides an anti-aging modified asphalt waterproofing membrane and a preparation method thereof.

[0005] In the first aspect, the present application provides an anti-aging modified asphalt waterproofing membrane, which adopts the following technical solution:

[0006] An anti-aging modified asphalt waterproofing coiled material comprises a polyester base fabric, a modified asphalt layer coated on the polyester base fabric and a polyethylene film covered on the modified asphalt layer, wherein the modified asphalt layer comprises the following raw materials in parts by weight: 42-48 parts of petroleum asphalt, 8-10 parts of base oil, 6-10 parts of SBS, 6-10 parts of SBR, 3-7 parts of terpene resin, 5-8 parts of anti-aging agent, 3-5 parts of light stabilizer, 5-7 parts of modified nano zeolite and 8-12 parts of modified nano montmorillonite.

[0007] By adopting the above technical scheme, the present application prepares an anti-aging waterproof membrane by mixing an anti-aging agent, a light stabilizer, a modified nano zeolite and a modified nano montmorillonite in petroleum asphalt. Compared with ordinary waterproof asphalt membrane, the anti-aging performance is significantly improved. At the same time, SBS is also added in the present application. SBS is blended with petroleum asphalt at high temperature. SBS can cause certain changes in the component composition of petroleum asphalt through swelling and adsorption. When SBS is dispersed in petroleum asphalt, the original colloidal structure balance in the petroleum asphalt is destroyed. SBS absorbs aromatics and colloids in the petroleum asphalt and swells to establish a new colloidal structure system. It forms an elastic network structure in the petroleum asphalt, which comprehensively improves the performance of the petroleum asphalt and improves the anti-aging performance of the asphalt waterproof membrane.

[0008] Modified nano zeolite and modified nano montmorillonite have large specific surface area and good adsorption performance. When asphalt waterproofing membrane begins to age, many lightweight small molecules will be produced. Modified nano zeolite and modified nano montmorillonite use their adsorption properties to firmly lock volatile small molecules, thereby enhancing the stability of asphalt waterproofing membrane. In addition, modified nano zeolite and modified nano montmorillonite can also be used as fillers to fill the gaps in asphalt waterproofing membrane, making the asphalt waterproofing membrane more compact, blocking the entry of oxygen and moisture, and further improving the anti-aging performance of asphalt waterproofing membrane.

[0009] In addition, nano zeolite added to asphalt has good high temperature resistance. After modification, the hydrophobicity of nano zeolite is adjusted, the surface energy is changed, the dispersibility of nano zeolite in asphalt and the compatibility with asphalt are enhanced, and the anti-aging performance of asphalt waterproofing membrane is improved; nano montmorillonite can form a relatively stable and uniform spatial network structure with SBS, improve the anti-aging performance of asphalt, and the modified nano montmorillonite has good compatibility with asphalt, which further improves the stability of asphalt waterproofing membrane.

[0010] At the same time, anti-aging agents, light stabilizers and SBS, modified nano zeolite and modified nano montmorillonite are added in this application to play an anti-aging role from different angles, exert a synergistic effect, and further improve the stability of the asphalt waterproof membrane.

[0011] To sum up, this application improves the anti-aging performance of asphalt waterproof membrane by adopting SBS modified petroleum asphalt, and further adds anti-aging agent, light stabilizer, modified nano zeolite and modified nano montmorillonite to mix and make anti-aging waterproof membrane. Compared with ordinary waterproof asphalt membrane, the anti-aging performance is significantly improved.

[0012] Preferably, the modified nano zeolite is prepared by the following method: dispersing the nano zeolite in water to form a suspension with a mass fraction of 6-10%, and ultrasonically dispersing for 15-20 minutes, then adding anhydrous ethanol solution of stearic acid to the suspension, stirring at a temperature of 50-90°C for 30-60 minutes, and then centrifuging at a speed of 2000-3500r / min for 5-8 minutes, filtering, and then drying at a temperature of 50-60°C for 20-24 hours, grinding, to obtain the modified nano zeolite, wherein the weight ratio of stearic acid to nano zeolite is 1: (20-30).

[0013] By adopting the above-mentioned technical scheme, the present application adopts stearic acid as a modifier to modify the nano zeolite. The surface treatment of the nano zeolite with stearic acid can improve the affinity of the zeolite with the asphalt base material and increase its dispersion in the asphalt. At the same time, it improves the compatibility between petroleum asphalt and other components, thereby improving the mechanical properties of the asphalt waterproofing membrane and improving its anti-aging performance.

[0014] Preferably, the modified nano-montmorillonite is prepared by the following method: dispersing the nano-montmorillonite in water to form a suspension with a mass fraction of 7-15%, stirring, then adding rosin-based quaternary ammonium salt to the suspension, stirring at a temperature of 40-50°C for 20-30min, filtering, and then drying at a temperature of 50-60°C for 20-24h, grinding, to obtain the modified nano-montmorillonite, wherein the weight ratio of the nano-montmorillonite to the rosin-based quaternary ammonium salt is 1: (42-45).

[0015] By adopting the above technical scheme, rosin-based quaternary ammonium salt is a natural cationic surfactant containing a phenanthrene ring structure, has good compatibility with asphalt, is a lipophilic group and has a lower critical micelle concentration and a lower surface tension, and thus has a stronger bactericidal power and higher surface activity and phase transfer catalytic ability than ordinary quaternary ammonium salts. Nano-montmorillonite has a "layered structure", and inserting rosin-based quaternary ammonium salt between the layers can effectively improve the affinity of nano-montmorillonite with asphalt base materials and improve its dispersion in asphalt, thereby improving the mechanical properties of waterproof membranes and improving the anti-aging properties of waterproof membranes.

[0016] Preferably, the mass ratio of the modified nano zeolite to the modified nano montmorillonite is 1:2.2.

[0017] Preferably, the anti-aging agent comprises maleic anhydride and polyphosphoric acid in a weight ratio of 1:(0.8-1.0).

[0018] By adopting the above technical scheme, the present application adopts a mixture of maleic anhydride and polyphosphoric acid, which can interact and improve the anti-aging performance of the modified asphalt waterproof membrane, thereby greatly extending the service life of the blue waterproof membrane.

[0019] Preferably, the light stabilizer comprises p-phenylenediamine and nano carbon black in a weight ratio of 1:(0.3-0.6).

[0020] By adopting the above technical scheme, p-phenylenediamine can terminate the generation of free radicals and inhibit the occurrence of free radical chain reactions during aging of the surface of waterproof asphalt membranes. Nano-carbon black has a very small particle size and a very large specific surface area, and is easily dispersed in the asphalt material to form a stable continuous phase. Nano-carbon black can adsorb free radicals generated during the thermal oxidative aging process and prevent the free radical chain reaction from proceeding, thereby further inhibiting the progress of thermal oxidative aging. The combination of p-phenylenediamine and nano-carbon black can significantly improve the anti-aging properties of modified asphalt waterproof membranes.

[0021] Preferably, the raw materials further include 0.3-0.8 parts by weight of dodecyl alcohol ester and 0.2-0.5 parts by weight of ethylene glycol.

[0022] By adopting the above-mentioned technical scheme, the present application adopts a mixture of dodecyl ester and ethylene glycol to jointly improve the film-forming properties of the asphalt waterproofing membrane and the density of the surface film, and improve the ability of the surface film to block the entry of oxygen and moisture into the interior of the waterproofing membrane, thereby improving the anti-aging properties of the modified asphalt waterproofing membrane, thereby greatly extending the service life of the asphalt waterproofing membrane.

[0023] Preferably, the mass ratio of the lauryl alcohol ester to ethylene glycol is 1:(1-1.3).

[0024] Preferably, the petroleum asphalt is 90# road asphalt.

[0025] In a second aspect, the present application provides a method for preparing an anti-aging modified asphalt waterproofing membrane, which adopts the following technical solution:

[0026] Step 1: Mix the base oil and petroleum asphalt according to the proportion, heat to 120-140°C, and stir for 50-60 minutes to obtain a mixture A;

[0027] Step 2: SBS, SBR, terpene resin, anti-aging agent and light stabilizer are mixed and melted in proportion to obtain a mixture B;

[0028] Step 3: Mixture A and mixture B are mixed, and stirred at a constant temperature of 140-150° C. for 60-80 min to obtain mixture C;

[0029] Step 4: adding the modified nano zeolite and the modified nano montmorillonite into the mixture C, stirring until they are evenly dispersed, and obtaining an anti-aging modified asphalt mixture;

[0030] Step 5: After the polyester base cloth is pre-impregnated, the anti-aging modified asphalt mixture is coated on the polyester base cloth, covered with a polyethylene film and cooled to form an anti-aging modified asphalt waterproof membrane.

[0031] By adopting the above technical scheme, the present application firstly mixes the petroleum asphalt and the base oil thoroughly to provide a good mixing basis for the remaining components, then melts the SBS, SBR, terpene resin, anti-aging agent and light stabilizer and mixes them thoroughly with the petroleum asphalt, and finally mixes them evenly with the modified nano zeolite and modified nano montmorillonite, and finally forms the anti-aging asphalt modified coil through coating, lamination and cooling and setting. The preparation method of the present application has simple steps, is easy to operate, and is suitable for large-scale industrial production.

[0032] In summary, this application has the following beneficial effects:

[0033] 1. Anti-aging agent, light stabilizer and SBS, modified nano zeolite and modified nano montmorillonite are added to the present application for use in combination, which play an anti-aging role from different angles. When the asphalt waterproofing membrane is about to age, a lot of light small molecules will be produced. The modified nano zeolite and modified nano montmorillonite use their adsorption properties to firmly lock the volatile small molecules, thereby enhancing the stability of the asphalt waterproofing membrane. In addition, the modified nano zeolite and modified nano montmorillonite can also be used as fillers to fill the gaps in the asphalt waterproofing membrane, making the asphalt waterproofing membrane more compact, blocking the entry of oxygen and moisture, and further improving the anti-aging performance of the asphalt waterproofing membrane;

[0034] 2. In the present application, by modifying nano zeolite and modified nano montmorillonite, the compatibility of nano particles with the system is improved, the mechanical properties of the prepared waterproof asphalt membrane are improved, and the anti-aging performance of the waterproof asphalt membrane is improved.

[0035] 3. The preparation method of the present application has simple steps, is easy to operate, and is suitable for large-scale industrial production. DETAILED DESCRIPTION

[0036] Source of raw materials:

[0037] Nano zeolite comes from Lingshou County Huimao Mineral Products Processing Plant;

[0038] Nano-montmorillonite comes from Lingshou County Huayao Mineral Products Processing Plant;

[0039] Nano calcium carbonate comes from Jingxian Jinxin Powder Co., Ltd.;

[0040] Stearic acid was from Guangzhou Shengli Chemical Co., Ltd., model 1801;

[0041] Mercaptopropyltriethoxysilane was from Nantong Runfeng Petrochemical Co., Ltd., model KH-580;

[0042] Rosin-based quaternary ammonium salt was from Hangzhou Tuomu Technology Co., Ltd., model A072;

[0043] Dodecyldimethylbenzylammonium bromide was from Wuhan Jiangxinyu Biotechnology Co., Ltd.;

[0044] Coking gas oil was from Shandong Shengxing Chemical Co., Ltd.;

[0045] SBS comes from Dongguan Yucheng Plastic Chemical Co., Ltd.;

[0046] SBR was from Shanghai Kaiyin Chemical Co., Ltd., model 1502;

[0047] Terpene resin was from Shanghai Kaiyin Chemical Co., Ltd.;

[0048] Polyphosphoric acid was from Shandong Jiaying Chemical Technology Co., Ltd.;

[0049] Nano carbon black comes from Lingshou County Yaxu Mineral Products Processing Plant.

[0050] Preparation Example

[0051] Preparation Example 1

[0052] The modified nano zeolite is prepared by the following method:

[0053] 6 kg of nano zeolite was dispersed in water to form a suspension with a mass fraction of 6%, and ultrasonically dispersed for 15 minutes. Then, 3 kg of anhydrous ethanol solution of stearic acid with a mass fraction of 10% was added to the suspension, stirred at 50°C for 30 minutes, centrifuged at 2000 r / min for 5 minutes, filtered, and then dried at 50°C for 20 hours and ground to obtain modified nano zeolite.

[0054] Preparation Example 2

[0055] The modified nano zeolite is prepared by the following method:

[0056] 6 kg of nano zeolite was dispersed in water to form a suspension with a mass fraction of 10%, and ultrasonically dispersed for 20 minutes. Then, 2 kg of anhydrous ethanol solution of stearic acid with a mass fraction of 10% was added to the suspension, stirred at 90°C for 60 minutes, and then centrifuged at 3500 r / min for 8 minutes, filtered, and then dried at 60°C for 24 hours and ground to obtain modified nano zeolite.

[0057] Preparation Example 3

[0058] The difference between Preparation Example 3 and Preparation Example 2 is that the nano zeolite is modified by a silane coupling agent. The specific steps are as follows: take 6 kg of nano zeolite, add 25 L of toluene and 3 kg of mercaptopropyltriethoxysilane, stir at 120°C for 11 hours, wash three times with ethanol, let stand and precipitate, pour off the supernatant, and dry the nano zeolite at 120°C for 6 hours to obtain a zeolite modified by a silane coupling agent.

[0059] Preparation Example 4

[0060] The modified nano-montmorillonite was prepared by the following method: 4.2 kg of nano-montmorillonite was dispersed in water to form a suspension with a mass fraction of 7%, stirred, and then 0.1 kg of rosin-based quaternary ammonium salt was added to the suspension, stirred at a temperature of 40°C for 20 minutes, filtered, and then dried at a temperature of 50°C for 20 hours, and ground to obtain the modified nano-montmorillonite.

[0061] Preparation Example 5

[0062] The modified nano-montmorillonite was prepared by the following method: 4.5 kg of nano-montmorillonite was dispersed in water to form a suspension with a mass fraction of 15%, stirred, and then 0.1 kg of rosin-based quaternary ammonium salt was added to the suspension, stirred at a temperature of 50°C for 30 minutes, filtered, and then dried at a temperature of 60°C for 24 hours, and ground to obtain the modified nano-montmorillonite.

[0063] Preparation Example 6

[0064] The difference between Preparation Example 6 and Preparation Example 5 is that the rosin-based quaternary ammonium salt is replaced by dodecyl dimethyl benzyl ammonium bromide, and the remaining steps are the same. Example

[0065] Example 1

[0066] An anti-aging modified asphalt waterproofing membrane comprises the following preparation steps:

[0067] Step 1: Add 8kg coking wax oil and 42kg 90# road asphalt into the batching tank, heat to 120℃, and stir for 50min.

[0068] Step 2: 6 kg SBS, 6 kg SBR, 3 kg terpene resin, 5 kg anti-aging agent (2.78 kg maleic anhydride and 2.23 kg polyphosphoric acid) and 3 kg light stabilizer (2.31 kg p-phenylenediamine and 0.69 kg nano carbon black) were added into a twin-screw extruder for melting.

[0069] Step 3: extruding the melted SBS, SBR, terpene resin, anti-aging agent and light stabilizer into the batching tank of step 1;

[0070] Step 4: Stir at a constant temperature of 140°C for 60 minutes.

[0071] Step 5: The mixture obtained in step 4 is kept at a constant temperature of 140° C., 5 kg of modified nano zeolite (from preparation example 1) and 8 kg of modified nano montmorillonite (from preparation example 4) are added to the mixture obtained in step 4, and stirred until uniformly dispersed to obtain an anti-aging modified asphalt mixture;

[0072] Step 6: Put the anti-aging modified asphalt mixture obtained in step 5 into the oil coating pool, and coat the anti-aging modified asphalt mixture on the polyester base cloth after pre-impregnation. The thickness of the anti-aging modified asphalt mixture is 3mm. After covering with a polyethylene film, cool and shape it to obtain an anti-aging modified asphalt waterproof membrane.

[0073] Example 2

[0074] An anti-aging modified asphalt waterproofing membrane comprises the following preparation steps:

[0075] Step 1: Add 9kg coking wax oil and 45kg 90# road asphalt into the batching tank, heat to 130℃, and stir for 55min.

[0076] Step 2: 8kg SBS, 8kg SBR, 5kg terpene resin, 7kg anti-aging agent (3.89kg maleic anhydride and 3.11kg polyphosphoric acid) and 4kg light stabilizer (3.08kg p-phenylenediamine and 0.92kg nano carbon black) were added into a twin-screw extruder for melting.

[0077] Step 3: extruding the melted SBS, SBR, terpene resin, anti-aging agent and light stabilizer into the batching tank of step 1;

[0078] Step 4: Stir at a constant temperature of 145°C for 70 minutes.

[0079] Step 5: The mixture obtained in step 4 is kept at a constant temperature of 145° C., 6 kg of modified nano zeolite (from preparation example 1) and 10 kg of modified nano montmorillonite (from preparation example 4) are added to the mixture obtained in step 4, and stirred until uniformly dispersed to obtain an anti-aging modified asphalt mixture;

[0080] Step 6: Put the anti-aging modified asphalt mixture obtained in step 5 into the oil coating pool, and coat the anti-aging modified asphalt mixture on the polyester base cloth after pre-impregnation. The thickness of the anti-aging modified asphalt mixture is 3mm. After covering with a polyethylene film, cool and shape it to obtain an anti-aging modified asphalt waterproof membrane.

[0081] Example 3

[0082] An anti-aging modified asphalt waterproofing membrane comprises the following preparation steps:

[0083] Step 1: Add 10kg coking wax oil and 48kg 90# road asphalt into the batching tank, heat to 140℃, and stir for 60min.

[0084] Step 2: 10kg SBS, 10kg SBR, 7kg terpene resin, 5kg anti-aging agent (2.78kg maleic anhydride and 2.22kg polyphosphoric acid, mass ratio 1:0.8) and 5kg light stabilizer (3.85kg p-phenylenediamine and 1.15kg nano carbon black, mass ratio 1:0.3) were added into a twin-screw extruder for melting.

[0085] Step 3: extruding the melted SBS, SBR, terpene resin, anti-aging agent and light stabilizer into the batching tank of step 1;

[0086] Step 4: Stir at a constant temperature of 150°C for 80 minutes.

[0087] Step 5: The mixture obtained in step 4 is kept at a constant temperature of 150° C., 7 kg of modified nano zeolite (from preparation example 1) and 12 kg of modified nano montmorillonite (from preparation example 4) are added to the mixture obtained in step 4, and stirred until uniformly dispersed to obtain an anti-aging modified asphalt mixture;

[0088] Step 6: Put the anti-aging modified asphalt mixture obtained in step 5 into the oil coating pool, and coat the anti-aging modified asphalt mixture on the polyester base cloth after pre-impregnation. The thickness of the anti-aging modified asphalt mixture is 3mm. After covering with a polyethylene film, cool and shape it to obtain an anti-aging modified asphalt waterproof membrane.

[0089] Example 4

[0090] An anti-aging modified asphalt waterproofing membrane is different from Example 3 in that the modified nano zeolite in step 5 comes from Preparation Example 2, and the remaining steps are the same as Example 3.

[0091] Example 5

[0092] An anti-aging modified asphalt waterproofing membrane is different from Example 3 in that the modified nano zeolite in step 5 comes from Preparation Example 3, and the remaining steps are the same as Example 3.

[0093] Example 6

[0094] An anti-aging modified asphalt waterproofing membrane is different from Example 3 in that nano-montmorillonite is modified in step 5 to prepare Example 5, and the remaining steps are the same as Example 3.

[0095] Example 7

[0096] An anti-aging modified asphalt waterproofing membrane is different from Example 3 in that nano-montmorillonite is modified in step 5 to prepare Example 6, and the remaining steps are the same as Example 3.

[0097] Example 8

[0098] An anti-aging modified asphalt waterproofing membrane is different from Example 6 in that the modified nano-montmorillonite is 14 kg, the mass ratio of the modified nano-zeolite to the modified nano-montmorillonite is 1:2, and the remaining steps are the same as Example 6.

[0099] Example 9

[0100] An anti-aging modified asphalt waterproofing membrane is different from Example 6 in that the modified nano-montmorillonite is 14.7 kg, the mass ratio of the modified nano-zeolite to the modified nano-montmorillonite is 1:2.1, and the remaining steps are the same as Example 6.

[0101] Example 10

[0102] An anti-aging modified asphalt waterproofing membrane is different from Example 6 in that the modified nano-montmorillonite is 15.4 kg, the mass ratio of the modified nano-zeolite to the modified nano-montmorillonite is 1:2.2, and the remaining steps are the same as Example 6.

[0103] Embodiment 11

[0104] An anti-aging modified asphalt waterproofing membrane is different from Example 6 in that the modified nano-montmorillonite is 16.1 kg, the mass ratio of the modified nano-zeolite to the modified nano-montmorillonite is 1:2.3, and the remaining steps are the same as Example 6.

[0105] Example 12

[0106] An anti-aging modified asphalt waterproof membrane is different from Example 10 in that, in the anti-aging agent, maleic anhydride is 2.94 kg, polyphosphoric acid is 2.06 kg, the mass ratio of maleic anhydride to polyphosphoric acid is 1:0.7, and the remaining steps are the same as Example 10.

[0107] Example 13

[0108] An anti-aging modified asphalt waterproof membrane is different from Example 10 in that, in the anti-aging agent, maleic anhydride is 2.63 kg, polyphosphoric acid is 2.37 kg, the mass ratio of maleic anhydride to polyphosphoric acid is 1:0.9, and the remaining steps are the same as Example 10.

[0109] Embodiment 14

[0110] An anti-aging modified asphalt waterproofing membrane is different from Example 10 in that, in the anti-aging agent, maleic anhydride is 2.5 kg, polyphosphoric acid is 2.5 kg, the mass ratio of maleic anhydride to polyphosphoric acid is 1:1, and the remaining steps are the same as Example 10.

[0111] Embodiment 15

[0112] An anti-aging modified asphalt waterproofing membrane is different from Example 10 in that, in the anti-aging agent, maleic anhydride is 2.38 kg, polyphosphoric acid is 2.62 kg, the mass ratio of maleic anhydride to polyphosphoric acid is 1:1.1, and the remaining steps are the same as Example 10.

[0113] Example 16

[0114] An anti-aging modified asphalt waterproof membrane is different from Example 13 in that zinc oxide replaces the diphenylamine in the light stabilizer, and the remaining steps are the same as Example 13.

[0115] Embodiment 17

[0116] An anti-aging modified asphalt waterproof membrane is different from Example 13 in that zinc oxide replaces the nano carbon black in the light stabilizer, and the remaining steps are the same as Example 13.

[0117] Embodiment 18

[0118] An anti-aging modified asphalt waterproof membrane is different from Example 13 in that, in the light stabilizer, p-phenylenediamine is 4.17 kg, nano-carbon black is 0.83 kg, the mass ratio of p-phenylenediamine to nano-carbon black is 1:0.2, and the remaining steps are the same as Example 13.

[0119] Embodiment 19

[0120] An anti-aging modified asphalt waterproof membrane is different from Example 13 in that, in the light stabilizer, p-phenylenediamine is 3.45 kg, nano-carbon black is 1.55 kg, the mass ratio of p-phenylenediamine to nano-carbon black is 1:0.45, and the remaining steps are the same as Example 13.

[0121] Embodiment 20

[0122] An anti-aging modified asphalt waterproof membrane is different from Example 13 in that, in the light stabilizer, p-phenylenediamine is 3.13 kg, nano-carbon black is 1.87 kg, the mass ratio of p-phenylenediamine to nano-carbon black is 1:0.6, and the remaining steps are the same as Example 13.

[0123] Embodiment 21

[0124] An anti-aging modified asphalt waterproof membrane is different from Example 13 in that, in the light stabilizer, p-phenylenediamine is 2.94 kg, nano carbon black is 2.06 kg, the mass ratio of p-phenylenediamine to nano carbon black is 1:0.7, and the remaining steps are the same as Example 13.

[0125] Embodiment 22

[0126] An anti-aging modified asphalt waterproof membrane is different from Example 20 in that 0.3 kg of dodecyl alcohol ester and 0.2 kg of ethylene glycol are also added in step 2, and the remaining steps are the same as Example 20.

[0127] Embodiment 23

[0128] An anti-aging modified asphalt waterproof membrane is different from Example 20 in that 0.5 kg of dodecyl alcohol ester and 0.35 kg of ethylene glycol are also added in step 2, and the remaining steps are the same as Example 20.

[0129] Embodiment 24

[0130] An anti-aging modified asphalt waterproof membrane is different from Example 20 in that 0.8 kg of dodecyl alcohol ester and 0.5 kg of ethylene glycol are also added in step 2, and the remaining steps are the same as Example 20.

[0131] Embodiment 25

[0132] An anti-aging modified asphalt waterproof membrane, which is different from Example 24 in that 0.8 kg of dodecyl alcohol ester and 0.8 kg of ethylene glycol are also added in step 2, and the mass ratio of dodecyl alcohol ester to ethylene glycol is 1:1. The remaining steps are the same as Example 24.

[0133] Embodiment 26

[0134] An anti-aging modified asphalt waterproof membrane is different from Example 24 in that 0.8 kg of dodecyl alcohol ester and 0.96 kg of ethylene glycol are also added in step 2, and the mass ratio of dodecyl alcohol ester to ethylene glycol is 1:1.2. The remaining steps are the same as Example 24.

[0135] Embodiment 27

[0136] An anti-aging modified asphalt waterproof membrane is different from Example 24 in that 0.8 kg of dodecyl alcohol ester and 1.04 kg of ethylene glycol are also added in step 2, and the mass ratio of dodecyl alcohol ester to ethylene glycol is 1:1.3. The remaining steps are the same as Example 24.

[0137] Embodiment 28

[0138] An anti-aging modified asphalt waterproof membrane is different from Example 24 in that 0.8 kg of dodecyl alcohol ester and 1.12 kg of ethylene glycol are also added in step 2, and the mass ratio of dodecyl alcohol ester to ethylene glycol is 1:1.4. The remaining steps are the same as Example 24.

[0139] Comparative Example

[0140] Comparative Example 1

[0141] The difference from Example 3 is that the modified nano zeolite and modified nano montmorillonite are replaced by an equal amount of nano titanium dioxide, and the other steps are the same.

[0142] Comparative Example 2

[0143] The difference from Example 3 is that the modified nano zeolite is replaced by modified nano calcium carbonate, and the modified nano calcium carbonate is prepared by modifying nano calcium carbonate using a silane coupling agent, and the modification method is the same as the method of Preparation Example 3 in this application.

[0144] Comparative Example 3

[0145] The difference from Example 3 is that the modified nano-montmorillonite is replaced by modified nano-calcium carbonate, and the modified nano-calcium carbonate is prepared by modifying nano-calcium carbonate using a silane coupling agent, and the modification method is the same as the method of Preparation Example 3 in this application.

[0146] Comparative Example 4

[0147] The difference from Example 3 is that no modified nano-montmorillonite is added, and the other steps are the same.

[0148] Comparative Example 5

[0149] The difference from Example 3 is that no modified nano zeolite is added, and the other steps are the same.

[0150] Comparative Example 6

[0151] The difference from Example 3 is that modified nano zeolite and modified nano montmorillonite are not added, and the other steps are the same.

[0152] Performance testing

[0153] The modified asphalt waterproofing membranes of Examples 1-28 and Comparative Examples 1-6 were subjected to heat aging treatment at 70° C. for 168 h. Then, their anti-seepage performance and tensile strain performance in the longitudinal / transverse directions were tested according to the relevant provisions of GB / T23457-2009. The results are shown in the following table.

[0154] Table 1 Performance test table of modified asphalt waterproof membranes prepared in Examples 1-28 and Comparative Examples 1-6 after heat aging treatment

[0155]

[0156] As can be seen from Table 1, after thermal aging, the modified asphalt waterproofing membranes prepared in Examples 1-3 of the present application have a tensile retention rate and an elongation retention rate of more than 90%, no cracks at -23°C, and the longitudinal / transverse tensile force can reach more than 1000 (N / mm), and the anti-seepage performance can meet the standard, indicating that the modified asphalt waterproofing membranes prepared in the present application have good anti-aging performance, and also have good mechanical properties and anti-seepage performance;

[0157] Combining the data of Examples 3-5 and Table 1, it can be seen that the modified asphalt waterproofing membrane prepared in Example 3 has good anti-aging properties and mechanical properties, that is, the modified nano zeolite prepared in Preparation Example 1 has good performance. Compared with the nano zeolite modified by the silane coupling agent, the nano zeolite modified by stearic acid can obtain a modified nano zeolite with better performance, which can effectively enhance the compatibility of the modified nano zeolite with the system, thereby changing the mechanical properties of the asphalt waterproofing membrane;

[0158] Combining the data of Example 3, Examples 6-7 and Table 1, it can be seen that the modified nano-montmorillonite prepared in Preparation Example 5 has good performance, and compared with the nano-montmorillonite modified with dodecyl dimethyl benzyl ammonium bromide, the synergistic effect between the nano-montmorillonite modified with rosin-based quaternary ammonium salt and SBS is better;

[0159] Combining the data of Example 6, Examples 8-11 and Table 1, it can be seen that the modified nano-montmorillonite of Example 10 has good performance, that is, when the mass ratio of modified nano-zeolite to modified nano-montmorillonite is 1:2.2, the prepared modified asphalt waterproofing membrane has good anti-aging performance and mechanical properties;

[0160] Combining the data of Example 10, Examples 12-15 and Table 1, it can be seen that when the mass ratio of maleic anhydride to polyphosphoric acid is 1:(0.8-1), the modified asphalt waterproofing membranes prepared in Examples 10 and 13-14 have good anti-aging properties and mechanical properties;

[0161] Combining the data of Example 13, Examples 15-21 and Table 1, it can be seen that the light stabilizer p-phenylenediamine and nano carbon black have a synergistic effect, and the asphalt waterproofing membrane prepared by co-adding them into the asphalt system has good anti-aging performance. In addition, when the mass ratio of p-phenylenediamine to nano carbon black is in the range of 1: (0.3-0.6), the prepared modified asphalt waterproofing membrane has good anti-aging performance and mechanical properties;

[0162] Combining the data of Example 20, Examples 22-28 and Table 1, it can be seen that the combination of dodecyl alcohol ester and ethylene glycol can improve the film-forming performance and surface film density of the asphalt waterproofing membrane, and improve the ability of the surface film to block oxygen and moisture from entering the waterproofing membrane, thereby improving the anti-aging performance of the modified asphalt waterproofing membrane, and when the mass ratio of dodecyl alcohol ester to ethylene glycol is 1: (1-1.3), the prepared modified asphalt waterproofing membrane has good anti-aging performance and mechanical properties;

[0163] Combining the data of Comparative Example 1 and Example 3, it can be seen that the asphalt waterproofing membrane prepared by modified nano zeolite and modified nano montmorillonite in the present application has better anti-aging performance and mechanical properties than the conventional asphalt waterproofing membrane prepared by titanium dioxide;

[0164] Combined with the data of Example 3 and Comparative Examples 2-6, it can be seen that the modified nano zeolite and modified nano montmorillonite used in the present application have a synergistic effect and effectively improve the anti-aging performance and mechanical properties of the asphalt waterproof membrane.

[0165] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An anti-aging modified asphalt waterproofing membrane, characterized in that: The invention comprises a polyester tire base cloth, a modified asphalt layer coated on the polyester tire base cloth and a polyethylene film coated on the modified asphalt layer, wherein the modified asphalt layer comprises the following raw materials in parts by weight: 42-48 parts of petroleum asphalt, 8-10 parts of base oil, 6-10 parts of SBS, 6-10 parts of SBR, 3-7 parts of terpene resin, 5-8 parts of anti-aging agent, 3-5 parts of light stabilizer, 5-7 parts of modified nano zeolite and 8-12 parts of modified nano montmorillonite; The modified nano zeolite is prepared by the following method: the nano zeolite is dispersed in water to form a suspension with a mass fraction of 6-10%, and ultrasonically dispersed for 15-20 minutes, and then a stearic acid anhydrous ethanol solution is added to the suspension, stirred at a temperature of 50-90° C. for 30-60 minutes, and then centrifuged at a speed of 2000-3500 r / min for 5-8 minutes, filtered, and then dried at a temperature of 50-60° C. for 20-24 hours, and ground to obtain the modified nano zeolite, wherein the weight ratio of stearic acid to nano zeolite is 1: (20-30); The modified nano-montmorillonite is prepared by the following method: dispersing the nano-montmorillonite in water to form a suspension with a mass fraction of 7-15%, stirring, then adding rosin-based quaternary ammonium salt to the suspension, stirring at a temperature of 40-50°C for 20-30 minutes, filtering, and then drying at a temperature of 50-60°C for 20-24 hours, grinding, and obtaining the modified nano-montmorillonite, wherein the weight ratio of the nano-montmorillonite to the rosin-based quaternary ammonium salt is 1: (42-45).

2. The anti-aging modified asphalt waterproofing membrane according to claim 1, characterized in that: The mass ratio of the modified nano zeolite to the modified nano montmorillonite is 1:2.

2.

3. The anti-aging modified asphalt waterproofing membrane according to claim 1, characterized in that: The anti-aging agent includes maleic anhydride and polyphosphoric acid in a weight ratio of 1:(0.8-1.0).

4. The anti-aging modified asphalt waterproofing membrane according to claim 1, characterized in that: The light stabilizer comprises p-phenylenediamine and nano carbon black in a weight ratio of 1:(0.3-0.6).

5. The anti-aging modified asphalt waterproofing membrane according to claim 1, characterized in that: The modified asphalt layer raw material also includes 0.3-0.8 parts by weight of dodecyl alcohol ester and 0.2-0.5 parts by weight of ethylene glycol.

6. The anti-aging modified asphalt waterproofing membrane according to claim 5, characterized in that: The mass ratio of the lauryl alcohol ester to ethylene glycol is 1:(1-1.3).

7. The anti-aging modified asphalt waterproofing membrane according to claim 1, characterized in that: The petroleum asphalt adopts 90# road asphalt.

8. A method for preparing the anti-aging modified asphalt waterproofing membrane according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: Step 1: mixing base oil and petroleum asphalt according to the proportion, heating to 120-140° C., and stirring for 50-60 minutes to obtain a mixture A; Step 2: SBS, SBR, terpene resin, anti-aging agent and light stabilizer are mixed and melted in proportion to obtain a mixture B; Step 3: Mixture A and mixture B are mixed, and stirred at a constant temperature of 140-150° C. for 60-80 min to obtain mixture C; Step 4: adding the modified nano zeolite and the modified nano montmorillonite into the mixture C, stirring until they are evenly dispersed, and obtaining an anti-aging modified asphalt mixture; Step 5: After the polyester base cloth is pre-impregnated, the anti-aging modified asphalt mixture is coated on the polyester base cloth, and then covered with a polyethylene film and cooled and shaped to obtain an anti-aging modified asphalt waterproof membrane.