Roof waterproof heat insulation coiled material and preparation method thereof

The roof waterproof and heat-insulating material addresses poor thermal performance and water absorption issues by incorporating foamed polyurethane with phase change materials and enhanced waterproof layers, providing dynamic temperature regulation and improved durability.

CN119062066AInactive Publication Date: 2024-12-03YUNNAN XINCHENG WATERPROOF TECH CO LTD

Patent Information

Application Number
CN202411272605.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional PVC and PE materials used for waterproofing and insulation rely on thermal conductivity for insulation, leading to poor thermal performance under extreme climate conditions and high water absorption, causing temperature fluctuations and material degradation.

Method used

A roof waterproof and heat-insulating material composed of a base layer, heat-insulating layer, waterproof layer, and diaphragm layer, where the heat-insulating layer incorporates a composite of foamed polyurethane and phase change materials like polyethylene glycol, paraffin, or fatty acid, with a modified polymer substrate and enhanced waterproof layers using nano materials.

Benefits of technology

The material achieves dynamic temperature regulation, reduces thermal conductivity, enhances mechanical strength, and improves durability and longevity by using phase change materials and modified polymers, maintaining structural integrity under various environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119062066A_ABST
    Figure CN119062066A_ABST
Patent Text Reader

Abstract

The invention relates to the field of waterproof heat insulation materials, and discloses a roof waterproof heat insulation coiled material and a preparation method thereof.The coiled material comprises a base layer, a heat insulation layer, a waterproof layer, a bonding layer and a diaphragm layer which are sequentially connected; wherein the heat insulation layer is formed by compounding foamed polyurethane and a phase change material, and the raw materials of the foamed polyurethane comprise polyether polyol, diphenylmethane diisocyanate, toluene diisocynate and a hydroxyl-containing flame retardant; the mass ratio of the diphenylmethane diisocyanate to the toluene diisocynate is 1: (1.5-3.5), the mass ratio of the polyether polyol to the hydroxyl-containing flame retardant is 10: (1-4), the phase-change material is selected from polyethylene glycol, paraffin or fatty acid, and the mass of the phase-change material accounts for 10%-30% of that of the thermal insulation layer. By introducing the phase change material (such as polyethylene glycol, paraffin and fatty acid) into the heat insulation layer of the coiled material, compared with a traditional polymer base material in the prior art, dynamic temperature adjustment can be achieved, and the heat insulation performance of the material is optimized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of waterproof and heat-insulating materials, in particular to a roof waterproof and heat-insulating coiled material and a preparation method thereof. Background Art

[0002] The waterproof material product made by impregnating asphalt or polymer waterproof materials on the carcass is provided in the form of a roll, which is called waterproof roll. According to the main component materials, it is divided into asphalt waterproof roll, polymer modified asphalt waterproof roll and synthetic polymer waterproof roll; according to the different carcasses, it is divided into carcass-free roll, paper carcass roll, glass fiber carcass roll, glass cloth carcass roll and polyethylene carcass roll. Waterproof roll is mainly used in building walls, roofs, tunnels, roads, landfills and other places. It is a flexible building material product that can be rolled into a roll to resist leakage of external rainwater and groundwater. As a leak-free connection between the engineering foundation and the building, it is the first barrier to waterproofing the entire project and plays a vital role in the entire project. The waterproof roll is required to have good water resistance, stability to temperature changes (no flow, no bubbling, no vibration at high temperatures; no brittle cracking at low temperatures), certain mechanical strength, elongation and fracture resistance, and certain flexibility and aging resistance.

[0003] In the prior art, coiled materials mainly rely on the thermal conductivity of the material itself for insulation. Although traditional PVC and PE materials have a certain thermal insulation effect, their thermal conductivity is relatively high. Under extreme climate conditions of high temperature or cold, their thermal insulation performance is poor and they cannot effectively regulate the temperature inside the building, resulting in large fluctuations in indoor temperature, increasing the air-conditioning load of the building, and thus increasing energy consumption.

[0004] Traditional PVC and PE materials have high water absorption rates, so they are prone to water absorption, expansion, and performance degradation in humid or long-term water-immersion environments. This water absorption will cause the thermal insulation performance of the coil to decrease, and may also cause damage to the internal structure of the material, shortening its service life.

[0005] Based on the above problems, the present invention provides a roof waterproof and heat-insulating coiled material and a preparation method thereof. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides a roof waterproof and heat-insulating roll material and a preparation method thereof, which solves the problem that the roll material mainly relies on the thermal conductivity of the material itself for heat insulation. Although traditional PVC and PE materials have a certain heat insulation effect, their thermal conductivity is relatively high, and their heat insulation performance is poor under extreme climate conditions of high temperature or cold.

[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions: a roof waterproof and heat-insulating roll material and a preparation method thereof, comprising a base layer, a heat-insulating layer, a waterproof layer, an adhesive layer and a diaphragm layer connected in sequence; wherein the heat-insulating layer is formed by a composite of foamed polyurethane and a phase change material, and the raw materials of the foamed polyurethane include polyether polyol, diphenylmethane diisocyanate, toluene diisocyanate and a hydroxyl-containing flame retardant; the mass ratio of diphenylmethane diisocyanate to toluene diisocyanate is 1:(1.5-3.5), the mass ratio of the polyether polyol to the hydroxyl-containing flame retardant is 10:(1-4), the phase change material is selected from polyethylene glycol, paraffin or fatty acid, and the mass of the phase change material accounts for 10%-30% of the heat-insulating layer.

[0008] Specifically, for the raw materials of the foamed polyurethane, when selecting polyether polyol, polybutylene glycol is preferably used as the base material, and this polyether polyol has high flexibility and chemical corrosion resistance. Diphenylmethane diisocyanate (MDI) and toluene diisocyanate (TDI) use a combined isocyanate, and the specific ratio is adjusted according to the application environment of the material. The weight average molecular weight of the polyether polyol is preferably in the range of 2000-4000 to ensure the flexibility and strength of the final foamed product and control the uniformity of the pores during the foaming process. The hydroxyl-containing flame retardant is preferably pentaerythritol phosphate, and its structural stability helps to improve the flame retardancy of the thermal insulation layer.

[0009] Preferably, the polyether polyol has a hydroxyl value of 26.5 mgKOH / g-117 mgKOH / g and a molecular weight of 2000-4000; the hydroxyl-containing flame retardant includes pentaerythritol phosphate, 2,2-bis(3-amino-4-hydroxyphenyl)-hexafluoropropane and 1,4-bis(dimethylhydroxysilyl)benzene.

[0010] Specifically, when the mixture of the polyether polyol and the hydroxyl-containing flame retardant is uniformly mixed in the reactor, a double-layer stainless steel reactor is preferably used. The equipment is equipped with an accurate temperature control system, and the temperature error is controlled within ±1°C. At the same time, a gas mixing system is equipped to maintain an inert atmosphere in the system by introducing nitrogen to avoid side reactions during the reaction. The reaction time is precisely controlled according to the amount and ratio of the reactants, preferably 30-60 minutes, and the temperature and pressure changes in the reactor are monitored in real time by an online monitoring system.

[0011] Preferably, the auxiliary materials of the foamed polyurethane include tri(cyclohexa-2,5-diene-1-yl)silane, a chain extender and a catalyst; wherein the amount of tri(cyclohexa-2,5-diene-1-yl)silane is 3%-7% of the mass of the main material of the foamed polyurethane, the chain extender is ethylene glycol, and the catalyst includes an organic metal catalyst, an amine catalyst and an acidic catalyst or a combination of the two.

[0012] Specifically, when the auxiliary materials of the foamed polyurethane include tri(cyclohexa-2,5-diene-1-yl)silane, it is recommended to be processed by a specific addition method. Tri(cyclohexa-2,5-diene-1-yl)silane is added in the initial stage of the foaming reaction to ensure its uniform distribution in the polyurethane matrix. At the same time, the amount of chain extender ethylene glycol added is regulated according to the final hardness and flexibility requirements of the foamed material. Preferably, the mass of the chain extender accounts for 2%-5% of the total amount of the foamed material. The catalyst preferably uses an organic metal catalyst and is mixed with an amine catalyst to form a dual catalytic system to increase the reaction rate.

[0013] Preferably, the waterproof layer comprises a nano waterproof coating composed of nano silicon dioxide, graphene or carbon nanotube material, and the thickness of the waterproof layer is 0.5 mm-2 mm.

[0014] Specifically, the thickness of the waterproof layer is controlled between 0.5mm and 2mm, and is enhanced by uniformly spraying a nano waterproof coating on the surface of the coil. The nano coating is composed of nano silicon dioxide, graphene or carbon nanotubes, and the particle size of the nanoparticles is preferably 10nm-50nm, ensuring the high hydrophobicity and high durability of the coating. The waterproof coating adopts ultrasonic spraying equipment, and the coating is evenly deposited on the surface of the material during the spraying process. The spraying thickness is maintained within 0.5μm-1μm through the precise control system of the equipment to ensure the uniformity and waterproof effect of the nano coating.

[0015] Preferably, the thickness of the tire base layer is less than 1.5 mm, the thickness of the diaphragm layer is 50 μm-100 μm, and the material of the diaphragm layer is selected from high-density polyethylene (HDPE) or polyvinylidene chloride (PVDC).

[0016] Specifically, the thickness of the tire base layer is further limited to less than 1.5 mm, and glass fiber or polyester fiber fabric is preferably used as the base material. Glass fiber fabric has higher heat resistance and tensile strength, and is suitable for use in high temperature environments. The thickness of the diaphragm layer is controlled between 50μm-100μm, and the diaphragm material is selected from high-density polyethylene (HDPE) or polyvinylidene chloride (PVDC), which can effectively block the penetration of water vapor and moisture. The diaphragm layer is adhered to the surface of the coil by a hot pressing process, and the hot pressing temperature is controlled between 100℃-150℃ to ensure close bonding between the material layers.

[0017] A method for preparing a roof waterproof and heat-insulating coiled material:

[0018] Mix diphenylmethane diisocyanate and toluene diisocyanate in a mass ratio of 1:(1.5-3.5), and heat to 60°C-80°C to completely melt them to obtain an isocyanate mixture;

[0019] The polyether polyol, hydroxyl-containing flame retardant, chain extender and catalyst are mixed in a reaction kettle according to a proportion, heated to 100°C-150°C, maintained at a vacuum degree of 100Pa-500Pa by a vacuum pump, reacted at a stirring speed of 500rpm-800rpm, and reacted for 30-90 minutes, and nitrogen was introduced for dehydration until the moisture content was less than 600ppm;

[0020] Gradually add the molten isocyanate mixture into the reaction kettle, continue stirring and reacting at 100°C-150°C for 30-60 minutes to form a foaming polyurethane prepolymer;

[0021] The foamed polyurethane prepolymer and the phase change material are mixed in proportion and preliminarily mixed by a single screw extruder at a temperature of 150°C to 180°C;

[0022] The preliminarily mixed foamed polyurethane and phase change material are secondary mixed in a twin-screw extruder, the screw diameter of the twin-screw extruder is 45mm-75mm, the screw aspect ratio is 30-40:1, the screw speed is 80rpm-150rpm, the material residence time is 2-5 minutes, and extruded and calendered to form a heat insulation layer sheet with a thickness of 5mm-60mm;

[0023] The heat insulation layer sheet and the tire base layer are compounded by a roller pressing compounding machine, the compounding temperature is 80℃-120℃, the compounding pressure is 5MPa-10MPa, and the compounding speed is 10m / min-30m / min. Then the waterproof layer, the adhesive layer and the diaphragm layer are coated to finally form a roll material.

[0024] Specifically, when the mixing and reaction steps in the preparation method are carried out in a reactor, the reactor is preferably designed with a double-layer jacket, equipped with an efficient stirring paddle inside, with a stirring speed of 500rpm-800rpm, and a cooling and heating system is set outside the reactor to accurately adjust the reaction temperature. After heating to 100°C-150°C, the gas in the reaction system is extracted by a vacuum pump, and the vacuum degree is preferably 100Pa-500Pa to ensure that no impurities enter during the reaction process and to ensure complete dehydration. The duration of the dehydration process is monitored in real time according to the moisture content of the reactants to ensure that the moisture content is less than 600ppm.

[0025] Preferably, the screw diameter of the single-screw extruder is 50 mm-100 mm, the aspect ratio is 25-30:1, and the accuracy of the temperature control system is ±2°C to ensure the mixing uniformity of the materials.

[0026] Specifically, when the foamed polyurethane and the phase change material are preliminarily mixed through a single screw extruder, the screw diameter of the extruder is preferably 50 mm-100 mm, and the screw structure adopts a step-by-step pressurization design to ensure that the material is gradually pressurized in the screw channel to eventually form a uniformly mixed material. During the extrusion process, the temperature is controlled at 150°C-180°C, and the temperature error of ±2°C is guaranteed by the temperature control system to ensure the uniformity of the mixing of the materials.

[0027] Preferably, during the composite process, an electrostatic adsorption device is used to perform surface treatment on the tire base layer, the electrostatic adsorption voltage is 10kV-20kV, and the composite tire base layer is polyester fiber or glass fiber fabric.

[0028] Specifically, in the composite process, an electrostatic adsorption device is used to perform surface treatment on the tire base layer. The adsorption voltage of the electrostatic adsorption device is 10kV-20kV. After the tire base layer is treated, the surface charge distribution is uniform, ensuring that the adhesion between the insulation layer sheet and the tire base layer is stable and firm. The composite tire base layer is preferably polyester fiber or glass fiber fabric to provide higher tensile strength and heat resistance. The composite speed is 10m / min-30m / min, and the composite pressure is controlled in real time by the servo system. The composite pressure is 5MPa-10MPa to ensure that the material is stably formed under high pressure.

[0029] Preferably, the mixture of foamable polyurethane and phase change material is foamed by a supercritical CO2 foaming process, the CO2 pressure is 30MPa-50MPa, the temperature is 80℃-100℃, and the foaming time is 30-120 minutes; the equipment used in the foaming process is a high-pressure reactor and a supercritical CO2 foaming device, the volume of the high-pressure reactor is 50L-200L, the operating pressure is 30MPa-60MPa, and it is equipped with a temperature control system with an accuracy of ±1℃; the foaming step includes: loading the mixture of foamable polyurethane and phase change material into the reactor, gradually increasing the pressure to the range of 30MPa-50MPa, and controlling the temperature at 80℃-100℃, maintaining this state for 30-120 minutes, and then completing the foaming process by quickly reducing the pressure to normal pressure.

[0030] Specifically, the mixture of foamed polyurethane and phase change material is foamed by a supercritical CO2 foaming process, the CO2 pressure is 30MPa-50MPa, the temperature is 80℃-100℃, and the foaming time is 30-120 minutes; the equipment used in the foaming process is a high-pressure reactor and a supercritical CO2 foaming device, the volume of the high-pressure reactor is 50L-200L, the operating pressure is 30MPa-60MPa, and it is equipped with a temperature control system with an accuracy of ±1℃; the foaming step includes: loading the mixture of foamed polyurethane and phase change material into the reactor, gradually increasing the pressure to the range of 30MPa-50MPa, and controlling the temperature at 80℃-100℃, maintaining this state for 30-120 minutes, and then completing the foaming process by quickly reducing the pressure to normal pressure.

[0031] Preferably, the thermal insulation layer sheet is cross-linked by γ-ray irradiation, the irradiation dose is 30kGy-100kGy, and the irradiation dose rate is 3kGy / min-6kGy / min, so as to ensure the structural stability of the material; the equipment used in the irradiation process is an industrial γ-ray irradiation device, the ray source is cobalt-60, the ray output power of the equipment is 500Ci-2000Ci, and an automatic transmission system is equipped to ensure that the thermal insulation layer sheet is uniformly irradiated; the irradiation step comprises: placing the prepared thermal insulation layer sheet on the conveyor belt of the irradiation device, the transmission speed is controlled at 5m / min-15m / min, the irradiation dose is controlled within the range of 30kGy-100kGy, and the irradiation dose rate is monitored in real time to ensure that the cross-linking of the material is fully completed.

[0032] Specifically, the thermal insulation layer sheet is cross-linked by γ-ray irradiation, the irradiation dose is 30kGy-100kGy, and the irradiation dose rate is 3kGy / min-6kGy / min to ensure the structural stability of the material; the equipment used in the irradiation process is an industrial γ-ray irradiation device, the ray source is cobalt-60, the ray output power of the equipment is 500Ci-2000Ci, and an automatic transmission system is equipped to ensure that the thermal insulation layer sheet is uniformly irradiated; the irradiation step includes: placing the prepared thermal insulation layer sheet on the conveyor belt of the irradiation device, the transmission speed is controlled at 5m / min-15m / min, the irradiation dose is controlled within the range of 30kGy-100kGy, and the irradiation dose rate is monitored in real time to ensure that the cross-linking of the material is fully completed.

[0033] The present invention provides a roof waterproof and heat-insulating coiled material and a preparation method thereof. The present invention has the following beneficial effects:

[0034] 1. The present invention introduces phase change materials (such as polyethylene glycol, paraffin, and fatty acids) into the insulation layer of the coil, which can achieve dynamic temperature regulation and optimize the thermal insulation performance of the material compared to the traditional polymer substrate in the prior art. The phase change material can absorb heat when the external temperature rises and maintain the internal temperature stable, and release the stored heat when the external temperature drops. This dynamic regulation mechanism greatly reduces the thermal conductivity of the coil. In addition, the present invention uses a modified polymer composite material with a low water absorption rate, which effectively reduces the water absorption of the coil in a humid environment, avoids the problem of performance degradation of the material after absorbing water, and greatly improves the service life of the coil when exposed to a humid or water environment for a long time.

[0035] 2. The present invention optimizes the molecular structure by modifying the polymer substrate, so that the coil material can significantly improve the elongation at break while maintaining high tensile strength, thereby enhancing the toughness and tensile strength of the material. Compared with ordinary polyethylene (PE) or polyvinyl chloride (PVC) used in the prior art, the coil material of the present invention has stronger tear resistance and ductility, reducing the risk of brittle fracture of the material under external force or environmental stress. In addition, by using supercritical CO2 foaming process and radiation cross-linking technology, the anti-aging performance of the coil material is significantly improved, and the material can still maintain its mechanical properties when exposed to high temperature, ultraviolet rays and humidity for a long time, extending its service life.

[0036] 3. The present invention introduces enhanced polyurethane composite materials and uses radiation cross-linking treatment to enable the coiled material to maintain its original physical properties and appearance during long-term outdoor use. Compared with traditional polyurethane materials, the enhanced polyurethane in the present invention will not crack or fade under long-term ultraviolet irradiation. This anti-ultraviolet ability significantly reduces aging damage on the surface of the material. In addition, the modified polymer material in the present invention shows good resistance to extreme climate conditions in weather resistance tests. Whether it is high temperature, low temperature, humid or dry environment, the coiled material can maintain good structural integrity and protective performance, which makes it have a wide range of application prospects in harsh outdoor environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings of the present invention specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Please refer to the attached Figure 1 :

[0040] Example 1: Preparation of waterproof and heat-insulating coiled material with polyethylene glycol as phase change material

[0041] Recipe preparation:

[0042] Polyether polyol: polytetramethylene glycol with a weight average molecular weight of 3000 and a hydroxyl value of 50 mgKOH / g was used.

[0043] MDI and TDI were mixed in a mass ratio of 1:2.

[0044] The phase change material is polyethylene glycol, the melting temperature is selected to be 28° C., and it accounts for 20% of the total mass of the thermal insulation layer.

[0045] The hydroxyl-containing flame retardant uses pentaerythritol phosphate, and its mass accounts for 3% of the total foaming material.

[0046] Isocyanate Melting:

[0047] The mixture of MDI and TDI was heated to 70°C and kept stirring until the mixture was completely melted and homogeneous.

[0048] Prepolymer reaction:

[0049] The polyether polyol was mixed with pentaerythritol phosphate, chain extender ethylene glycol and catalyst in a double-layer jacketed reactor and heated to 130°C.

[0050] Dehydrate under a vacuum condition of 500 Pa for 1 hour until the moisture content is less than 600 ppm.

[0051] The molten isocyanate mixture was gradually added under a stirring speed of 600 rpm, and the stirring reaction was continued for 45 minutes to form a foamed polyurethane prepolymer.

[0052] Mixture of Phase Change Materials:

[0053] The prepolymer was mixed with polyethylene glycol in a 20% ratio in a single screw extruder. The extruder temperature was controlled at 160°C, the screw diameter was 75 mm, and the screw aspect ratio was 30:1.

[0054] Twin screw extrusion:

[0055] The mixture was secondarily mixed in a twin-screw extruder with a screw speed of 100 rpm and a material residence time of 3 minutes.

[0056] The heat insulation layer sheet with a thickness of 30 mm was formed by extrusion and calendaring.

[0057] Composite process:

[0058] The base layer is made of glass fiber fabric with a thickness of 1 mm, which is compounded with the heat insulation layer sheet on a roller laminating machine. The compounding temperature is 100°C and the compounding pressure is 8 MPa.

[0059] Then, a waterproof layer with a thickness of 1 mm is coated on the composite sheet, using a nano-silicon dioxide coating, and the thickness is uniformly controlled at 1 μm.

[0060] Coil Forming:

[0061] Finally, a high-density polyethylene (HDPE) diaphragm layer with a thickness of 80 μm is covered on the adhesive layer through a hot pressing device. The hot pressing temperature is 120° C. and the pressure is 6 MPa. After molding, the final coil is obtained.

[0062] New content: This embodiment introduces the phase change material polyethylene glycol. By combining the phase change material with the foamed polyurethane, the thermal insulation performance can be actively adjusted when the ambient temperature changes, thereby achieving a dynamic thermal insulation effect. Polyethylene glycol has a low melting point and is suitable for use at room temperature, so it can greatly improve the thermal insulation capacity of the coil.

[0063] Compared with the prior art, this embodiment increases the thermal insulation flexibility of the coil by using phase change materials. Especially in an environment with a large temperature difference between day and night, the polyethylene glycol phase change material can absorb and release heat, thereby achieving the effect of stabilizing the internal temperature and improving the energy efficiency and comfort of the building.

[0064] Example 2: Preparation of waterproof and heat-insulating coiled material using paraffin as phase change material

[0065] Recipe preparation:

[0066] The polyether polyol is polybutylene glycol with a molecular weight of 4000 and a hydroxyl value of 30 mgKOH / g.

[0067] The mass ratio of MDI to TDI is 1:1.5.

[0068] The phase change material is paraffin, the melting temperature is 25°C, and the mass accounts for 15% of the total mass of the thermal insulation layer.

[0069] The hydroxy-containing flame retardant used was 2,2-bis(3-amino-4-hydroxyphenyl)-hexafluoropropane.

[0070] Isocyanate treatment:

[0071] The MDI and TDI mixture was heated to 65°C and kept stirring until completely dissolved.

[0072] Prepolymer reaction:

[0073] The polyether polyol was mixed with the flame retardant and the chain extender in a jacketed reactor, heated to 150°C, and stirred at 500 rpm.

[0074] Dehydration was performed under a vacuum condition of 300Pa for 1.5 hours to ensure that the moisture content was less than 500ppm.

[0075] The isocyanate mixture was gradually added and stirring was continued for 60 minutes to form a prepolymer.

[0076] Phase change material mixing:

[0077] The paraffin wax was processed by microencapsulation technology and mixed with the prepolymer in a single screw extruder with a screw diameter of 50 mm and an extrusion temperature of 170°C.

[0078] Twin-screw extrusion and calendering:

[0079] The screw speed of the twin-screw extruder is 90 rpm, the aspect ratio is 35:1, and the thermal insulation layer sheet with a thickness of 40 mm is formed by calendering.

[0080] Composite process:

[0081] The tire base layer uses a polyester fiber fabric with a thickness of 0.8 mm, a composite temperature of 90°C, and a pressure of 7 MPa.

[0082] The waterproof layer is made of graphene nano-coating with a spray thickness of 0.8mm.

[0083] Coil Forming:

[0084] The adhesive layer is covered with a PVDC separator, the hot pressing temperature is 130°C, the thickness of the separator layer is 60 μm, and the final coil is formed by roller pressing.

[0085] New content: Paraffin is added to the coil as a phase change material, and microencapsulation technology is used to encapsulate the paraffin, solving the problem of easy leakage and uneven distribution of phase change materials. In addition, graphene nano-coating is added as a waterproof layer, which greatly enhances the wear resistance and anti-aging performance of the coil.

[0086] By introducing microencapsulated paraffin and graphene waterproof coating, this embodiment shows stronger heat storage and insulation effect in low temperature environment compared with the prior art. Paraffin material can effectively absorb ambient heat in cold conditions and prolong indoor warmth time, which is particularly suitable for building waterproof and heat insulation needs in cold areas. At the same time, the graphene waterproof coating improves the waterproofness and service life of the coiled material.

[0087] Example 3: Preparation of waterproof and heat-insulating rolls using fatty acids as phase change materials

[0088] Recipe preparation:

[0089] The polyether polyol selected has a molecular weight of 2000 and a hydroxyl value of 45 mgKOH / g.

[0090] The mixing ratio of MDI and TD I is 1:3.

[0091] The phase change material is fatty acid, has a melting point of 30° C., and its mass accounts for 10% of the total mass of the thermal insulation layer.

[0092] The hydroxy-containing flame retardant used is 1,4-bis(dimethylhydroxysilyl)benzene.

[0093] Isocyanate Dissolution:

[0094] Heat MDI and TDI to 80 °C and stir continuously to ensure uniform mixing.

[0095] Prepolymer reaction:

[0096] The polyether polyol and the flame retardant were mixed in a reactor at a reaction temperature of 120°C.

[0097] Dehydration was carried out under a vacuum condition of 400 Pa, with a stirring speed of 600 rpm and a dehydration time of 1 hour.

[0098] Mixture of Phase Change Materials:

[0099] The fatty acid was mixed with the foaming prepolymer in a single screw extruder at an extruder temperature of 160°C and a screw length-to-diameter ratio of 25:1.

[0100] Twin-screw extrusion and calendering:

[0101] The twin-screw extruder has a screw diameter of 60 mm and a screw speed of 110 rpm, forming a heat insulation layer sheet with a thickness of 25 mm.

[0102] Composite process:

[0103] A glass fiber base layer with a thickness of 0.9 mm was selected, the composite temperature was 85°C, and the pressure was 6 MPa.

[0104] The waterproof layer is made of carbon nanotube material and the coating thickness is 1mm.

[0105] Coil Forming:

[0106] The adhesive layer is covered with a high-density polyethylene diaphragm, the hot pressing temperature is 140°C, the diaphragm thickness is 70μm, and the coil is shaped after cooling after molding.

[0107] New content: In this embodiment, fatty acid is used as a phase change material for the thermal insulation layer, which has a high melting point and is suitable for high temperature environments. By introducing carbon nanotubes as a waterproof coating, the waterproofness and mechanical strength of the coil are greatly improved, enabling it to withstand the harsh conditions in high temperature environments.

[0108] Compared with existing technologies, the use of fatty acid phase change materials enables the roll to maintain excellent thermal insulation performance in high temperature environments, which is suitable for the thermal insulation needs of buildings in tropical or high temperature areas. The application of carbon nanotubes significantly enhances the durability and tear resistance of the waterproof layer, making the roll have a longer service life in extreme weather conditions.

[0109] Example 4: Preparation of waterproof and heat-insulating membrane using supercritical CO2 foaming process

[0110] Recipe preparation:

[0111] The polyether polyol selected has a molecular weight of 3000 and a hydroxyl value of 55 mgKOH / g.

[0112] MDI and TDI were mixed in a ratio of 1:2.

[0113] The phase change material is polyethylene glycol, and its mass accounts for 25% of the total mass of the heat insulation layer.

[0114] Isocyanate Mixing and Handling:

[0115] The mixture of MDI and TDI was heated to 70°C and stirred until completely dissolved.

[0116] Prepolymer preparation:

[0117] The polyether polyol, the flame retardant and the chain extender are mixed in a reactor at a reaction temperature of 135°C.

[0118] The mixture was dehydrated under a vacuum of 500 Pa for 40 minutes, and then isocyanate was added and the reaction was continued for 50 minutes.

[0119] Phase change material mixing:

[0120] The foaming prepolymer was mixed with polyethylene glycol in a single screw extruder at an extrusion temperature of 165°C.

[0121] CO2 foaming process:

[0122] The supercritical CO2 foaming process is adopted, the CO2 pressure is 40MPa, the foaming temperature is 90°C, and the foaming time is 40 minutes.

[0123] Compounding and molding:

[0124] The tire base layer is a polyester fiber fabric with a thickness of 1.2 mm, the composite temperature is 100° C., and the composite pressure is 8 MPa.

[0125] The thickness of the nano-silica waterproof layer is 1 mm, the diaphragm layer is HDPE, and the hot pressing temperature is 130°C.

[0126] New content: This embodiment introduces a supercritical CO2 foaming process, replacing the traditional chemical foaming agent, making the foaming process more environmentally friendly. At the same time, the CO2 foaming process can control the uniformity of the pore structure, obtain a lighter foam material with better thermal insulation effect, and significantly reduce the weight of the coil.

[0127] Compared with existing technologies, supercritical CO2 foaming technology improves the uniformity of the pores and the thermal insulation performance of foamed polyurethane materials, and is particularly suitable for building applications that require lightweight thermal insulation materials. No harmful gases are produced during the foaming process, which meets environmental protection requirements, and the prepared thermal insulation layer material has better thermal stability and low thermal conductivity.

[0128] Example 5: Preparation of waterproof and heat-insulating coiled material cross-linked by gamma ray irradiation

[0129] Recipe preparation:

[0130] The polyether polyol selected has a molecular weight of 3500 and a hydroxyl value of 40 mgKOH / g.

[0131] MDI and TDI were mixed in a mass ratio of 1:1.

[0132] The phase change material is paraffin, and its mass accounts for 30% of the total mass of the thermal insulation layer.

[0133] Isocyanate treatment:

[0134] The isocyanate mixture was heated to 75°C and stirred to dissolve.

[0135] Prepolymer reaction:

[0136] The polyether polyol was reacted with the flame retardant at 150° C. and dehydrated for 60 minutes under vacuum conditions with a stirring speed of 500 rpm.

[0137] Phase change material mixing and extrusion:

[0138] The prepolymer and paraffin wax were mixed in a single screw extruder at an extrusion temperature of 170°C and a screw speed of 100 rpm.

[0139] Gamma irradiation cross-linking:

[0140] The heat insulation layer sheet is treated in a cobalt-60 irradiation device with an irradiation dose of 50 kGy, an irradiation dose rate of 4 kGy / min, and a treatment time of 20 minutes.

[0141] Compounding and molding:

[0142] The tire base layer is glass fiber with a thickness of 0.8 mm, the composite temperature is 85°C, the composite pressure is 7 MPa, the thickness of the diaphragm layer is 75 μm, and PVDC material is used.

[0143] New content: This embodiment adds gamma-ray irradiation cross-linking technology, which uses radiation to enhance the molecular cross-linking degree of the thermal insulation material, thereby increasing its heat resistance and UV resistance. Cobalt-60, as a ray source, can evenly irradiate the surface and interior of the material in a short time to achieve deep cross-linking treatment.

[0144] Compared with existing technologies, gamma-ray irradiation treatment makes the insulation layer material have higher structural stability and durability, suitable for long-term exposure to strong ultraviolet rays and high temperature environments. The coiled material after irradiation cross-linking can maintain a longer service life under extreme climatic conditions, which is particularly suitable for construction scenes that require high weather resistance.

[0145] Test experiment: The thermal insulation performance, water resistance, UV resistance, mechanical properties and weather resistance of the five embodiment coils were systematically tested to compare the comprehensive performance of different coils.

[0146] 1. Test purpose:

[0147] By testing the heat insulation, water resistance, UV resistance, mechanical properties and weather resistance of the coils of the five embodiments, the effects of phase change materials and foaming process on the performance of the coils were analyzed, and the optimal material combination and process parameters were determined.

[0148] 2. Test method:

[0149] 2.1 Thermal insulation performance test:

[0150] The heat flow method is used to test the thermal conductivity of the coil. During the test, the coil is fixed in a simulated building structure, and the temperature difference is measured on both sides of the coil using a thermocouple, and the heat flow under the stable temperature difference is recorded. The test conditions are set as follows:

[0151] The outdoor temperature is set to 45°C and maintained at a constant temperature.

[0152] The initial indoor temperature is 20℃.

[0153] The test time is 8 hours.

[0154] 2.2 Water resistance test:

[0155] Using the immersion test method, immerse the coil sample in water with a depth of 10 cm. Record the water absorption rate at different immersion times (24h, 48h, 72h), and observe the water seepage on the coil surface.

[0156] 2.3 UV resistance test:

[0157] Use a UV aging test chamber to simulate the exposure to ultraviolet rays in sunlight. Place the coil in the test chamber, set the UV intensity to a wavelength of 280nm-400nm, and irradiate for 500 hours. During this period, monitor whether the surface of the coil appears cracked, discolored, etc.

[0158] 2.4 Mechanical properties test:

[0159] The tensile strength and tear resistance of the coils were tested according to GB / T1040-92 standard, and the breaking strength and elongation of the coils were recorded. Each coil was tested 5 times and the average value was taken.

[0160] 2.5 Weather resistance test:

[0161] Use weathering test equipment to conduct accelerated aging tests on the coiled material under the combined effects of simulated wind, rain, heat and ultraviolet rays. Set the cycle test period to:

[0162] High temperature stage: 60℃, maintained for 8 hours;

[0163] Low temperature stage: -20℃, maintained for 8 hours;

[0164] Humidity stage: humidity 90%, maintained for 6 hours;

[0165] UV stage: UV intensity is 10W / m2, maintained for 5 hours.

[0166] Each cycle lasts for 27 hours in total, and the test is completed for 100 cycles (2700 hours) to check whether the coil has cracks, delamination, failure, etc.

[0167] 3. Test process:

[0168] Sample preparation: Coil samples with a specification of 300 mm×300 mm were cut from the five embodiments respectively, 10 samples were prepared for each coil, and five performance tests were performed.

[0169] Thermal insulation performance test: Conduct heat flow test in a constant temperature box and record thermal conductivity data.

[0170] Water resistance test: Put the sample into water and record the water absorption rate at 24h, 48h and 72h.

[0171] UV resistance test: Place the sample in a UV aging test chamber and record the surface condition of the coil after irradiation.

[0172] Mechanical property test: tensile and tearing tests were performed to obtain breaking strength and elongation.

[0173] Weathering test: Conduct accelerated weathering test and periodically check the appearance and structural changes of the coil.

[0174] 4. Experimental data table:

[0175]

[0176]

[0177] 5. Summary of test results:

[0178] Thermal insulation performance: The thermal conductivity of Examples 2 and 4 is relatively low, showing better thermal insulation effect. In particular, Example 4, due to the use of supercritical CO2 foaming process, has a more uniform cell structure, excellent thermal insulation effect, and a thermal conductivity of 0.029 W / m·K.

[0179] Water resistance: Example 4 exhibits the best water resistance, with a water absorption rate of only 0.5% after 72 hours. In comparison, the water absorption rates of Examples 1 and 3 are slightly higher, reaching 0.9% and 0.8% respectively.

[0180] UV resistance: All examples showed no obvious cracking or fading after 500 hours of UV irradiation, and only Example 2 showed a slight color change.

[0181] Mechanical properties: The mechanical properties of Example 4 are the most outstanding, with a tensile strength of 14.5 MPa and an elongation at break of 20.0%, which is due to the use of supercritical CO2 foaming and high-quality substrates, which enhance the structural strength of the material.

[0182] Weather resistance: After 100 weather resistance cycles, all examples showed no significant changes, no delamination, cracks or failure, proving that they are suitable for long-term applications in various harsh environments.

[0183] 6. Test experiment summary:

[0184] Through this experiment, the coils of the five embodiments were fully tested. Embodiment 4 showed the best comprehensive performance, especially in terms of thermal insulation, water resistance and mechanical properties, and was suitable for high-performance building requirements. Embodiment 2 performed well in low temperature environments, and the use of paraffin phase change materials made its heat storage effect better. The performance of embodiments 1, 3 and 5 was relatively balanced, and was suitable for waterproof and heat insulation applications in general buildings.

[0185] Experiment 1: Comprehensive comparison of thermal conductivity, water absorption and mechanical properties

[0186] Existing technical solutions

[0187] The existing technology uses traditional polyvinyl chloride (PVC) as the substrate, which has a high thermal conductivity and a high water absorption rate, resulting in a decrease in the performance of the material in a humid environment.

[0188] Technical solution of the present invention

[0189] The present invention adopts a modified polymer composite material, combining low thermal conductivity, low water absorption and excellent mechanical properties, aiming to improve the service life and stability of the material.

[0190] Experimental Procedure

[0191] Sample preparation: PVC samples according to the prior art and samples of the modified polymer composite material of the present invention were prepared respectively.

[0192] Thermal conductivity test: Use a thermal conductivity instrument to measure the thermal conductivity of the sample.

[0193] Water absorption test: Soak the sample in water for 24 hours, 48 ​​hours and 72 hours, and measure its water absorption.

[0194] Tensile strength and elongation at break test: Use a universal material testing machine to perform tensile tests and record the maximum tensile strength and elongation at break.

[0195] Data recording and analysis: record experimental data and conduct comparative analysis.

[0196] Experimental data table

[0197]

[0198]

[0199] Experiment 2: Multi-stage comparison of weather resistance and UV resistance

[0200] Existing technical solutions

[0201] The existing technology uses traditional polyurethane materials, which have good weather resistance but are prone to cracking and fading under ultraviolet rays.

[0202] Technical solution of the present invention

[0203] The invention adopts a reinforced polyurethane composite material, has excellent weather resistance and ultraviolet tolerance, and can effectively prevent cracking and fading.

[0204] Experimental Procedure

[0205] Sample preparation: The polyurethane samples of the prior art and the enhanced polyurethane samples of the present invention were prepared respectively.

[0206] UV resistance test: Place the sample in a UV irradiation device and observe cracking and fading after 500 hours.

[0207] Weathering test: Carry out weathering test under different climatic conditions and record the changes in different cycles (such as 100 hours, 200 hours, 300 hours).

[0208] Data recording and analysis: record experimental data and conduct comparative analysis.

[0209] Experimental data table

[0210]

[0211] Experiment 3: Comparison of comprehensive mechanical properties and aging properties

[0212] Existing technical solutions

[0213] The existing technology uses ordinary polyethylene (PE), which has a certain tensile strength, but in long-term use, the aging performance of the material is poor, which affects the service life.

[0214] Technical solution of the present invention

[0215] The invention adopts modified polymer materials, optimizes the molecular structure, enhances the tensile strength and elongation at break, and improves the aging performance.

[0216] Experimental Procedure

[0217] Sample preparation: PE samples of the prior art and modified polymer samples of the present invention were prepared respectively.

[0218] Tensile strength and elongation at break test: Use a universal material testing machine to perform tensile tests and record the maximum tensile strength and elongation at break.

[0219] Aging performance test: Place the sample in a high temperature and high humidity environment, and after different time periods (such as 100 hours, 200 hours, 300 hours), test the changes in tensile strength and elongation at break.

[0220] Data recording and analysis: record experimental data and conduct comparative analysis.

[0221] Experimental data table

[0222]

[0223] Summarize

[0224] Through the above three complex experimental designs, it can be clearly seen that the present invention has significant advantages over the prior art in multiple parameters (such as thermal conductivity, water absorption, tensile strength, elongation at break, weather resistance, UV tolerance and aging performance). These experimental data prove the superiority of the technical solution of the present invention in practical applications and can meet higher performance requirements.

[0225] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A roof waterproof and heat-insulating roll material, characterized in that: The coiled material includes a tire base layer, a heat-insulating layer, a waterproof layer, an adhesive layer and a diaphragm layer connected in sequence; wherein the heat-insulating layer is formed by a composite of foamed polyurethane and a phase change material, and the raw materials of the foamed polyurethane include polyether polyol, diphenylmethane diisocyanate, toluene diisocyanate and a hydroxyl-containing flame retardant; the mass ratio of diphenylmethane diisocyanate to toluene diisocyanate is 1:(1.5-3.5), the mass ratio of the polyether polyol to the hydroxyl-containing flame retardant is 10:(1-4), the phase change material is selected from polyethylene glycol, paraffin or fatty acid, and the mass of the phase change material accounts for 10%-30% of the heat-insulating layer.

2. A roof waterproof and heat-insulating roll material according to claim 1, characterized in that: The polyether polyol has a hydroxyl value of 26.5 mgKOH / g-117 mgKOH / g and a molecular weight of 2000-4000; the hydroxyl-containing flame retardant comprises pentaerythritol phosphate, 2,2-bis(3-amino-4-hydroxyphenyl)-hexafluoropropane and 1,4-bis(dimethylhydroxysilyl)benzene.

3. A roof waterproof and heat-insulating roll material according to claim 1, characterized in that: The auxiliary materials of the foamed polyurethane include tri(cyclohexa-2,5-diene-1-yl)silane, a chain extender and a catalyst; wherein the amount of tri(cyclohexa-2,5-diene-1-yl)silane is 3%-7% of the mass of the main material of the foamed polyurethane, the chain extender is ethylene glycol, and the catalyst includes an organic metal catalyst, an amine catalyst and an acid catalyst or a combination of the two.

4. A roof waterproof and heat-insulating roll material according to claim 1, characterized in that: The waterproof layer comprises a nano waterproof coating composed of nano silicon dioxide, graphene or carbon nanotube materials, and the thickness of the waterproof layer is 0.5mm-2mm.

5. The roof waterproof and heat-insulating coiled material according to claim 1, characterized in that: The thickness of the tire base layer is less than 1.5 mm, the thickness of the diaphragm layer is 50 μm-100 μm, and the material of the diaphragm layer is selected from high-density polyethylene (HDPE) or polyvinylidene chloride (PVDC).

6. A method for preparing a roof waterproof and heat-insulating coiled material, according to a roof waterproof and heat-insulating coiled material according to claims 1-5, characterized in that: Mix diphenylmethane diisocyanate and toluene diisocyanate in a mass ratio of 1:(1.5-3.5), and heat to 60°C-80°C to completely melt them to obtain an isocyanate mixture; The polyether polyol, hydroxyl-containing flame retardant, chain extender and catalyst are mixed in a reaction kettle according to a proportion, heated to 100°C-150°C, maintained at a vacuum degree of 100Pa-500Pa by a vacuum pump, reacted at a stirring speed of 500rpm-800rpm, and reacted for 30-90 minutes, and nitrogen was introduced for dehydration until the moisture content was less than 600ppm; Gradually add the molten isocyanate mixture into the reaction kettle, continue stirring and reacting at 100°C-150°C for 30-60 minutes to form a foaming polyurethane prepolymer; The foamed polyurethane prepolymer and the phase change material are mixed in proportion and preliminarily mixed by a single screw extruder at a temperature of 150°C to 180°C; The preliminarily mixed foamed polyurethane and phase change material are secondary mixed in a twin-screw extruder, the screw diameter of the twin-screw extruder is 45mm-75mm, the screw aspect ratio is 30-40:1, the screw speed is 80rpm-150rpm, the material residence time is 2-5 minutes, and extruded and calendered to form a heat insulation layer sheet with a thickness of 5mm-60mm; The heat insulation layer sheet and the tire base layer are compounded by a roller pressing compounding machine, the compounding temperature is 80℃-120℃, the compounding pressure is 5MPa-10MPa, and the compounding speed is 10m / min-30m / min. Then the waterproof layer, the adhesive layer and the diaphragm layer are coated to finally form a roll material.

7. A roof waterproof and heat-insulating coiled material and a preparation method thereof according to claim 6, characterized in that: The screw diameter of the single-screw extruder is 50mm-100mm, the aspect ratio is 25-30:1, and the accuracy of the temperature control system is ±2°C, ensuring the mixing uniformity of the materials.

8. A roof waterproof and heat-insulating coiled material and a preparation method thereof according to claim 6, characterized in that: During the composite process, an electrostatic adsorption device is used to perform surface treatment on the tire base layer, the electrostatic adsorption voltage is 10kV-20kV, and the composite tire base layer is polyester fiber or glass fiber fabric.

9. A roof waterproof and heat-insulating coiled material and a preparation method thereof according to claim 6, characterized in that: The mixture of foamable polyurethane and phase change material is foamed by a supercritical CO2 foaming process, the CO2 pressure is 30MPa-50MPa, the temperature is 80℃-100℃, and the foaming time is 30-120 minutes; the equipment used in the foaming process is a high-pressure reactor and a supercritical CO2 foaming device, the volume of the high-pressure reactor is 50L-200L, the operating pressure is 30MPa-60MPa, and it is equipped with a temperature control system with an accuracy of ±1℃; the foaming step includes: loading the mixture of foamable polyurethane and phase change material into the reactor, gradually increasing the pressure to the range of 30MPa-50MPa, and controlling the temperature at 80℃-100℃, maintaining this state for 30-120 minutes, and then completing the foaming process by quickly reducing the pressure to normal pressure.

10. A roof waterproof and heat-insulating coiled material and a preparation method thereof according to claim 6, characterized in that: The heat insulation layer sheet is cross-linked by γ-ray irradiation, the irradiation dose is 30kGy-100kGy, and the irradiation dose rate is 3kGy / min-6kGy / min, so as to ensure the structural stability of the material; the equipment used in the irradiation process is an industrial γ-ray irradiation device, the ray source is cobalt-60, the ray output power of the equipment is 500Ci-2000Ci, and an automatic transmission system is equipped to ensure that the heat insulation layer sheet is evenly irradiated; The irradiation step includes: placing the prepared insulation layer sheet on the conveyor belt of the irradiation device, controlling the transmission speed within 5m / min-15m / min, controlling the irradiation dose within the range of 30kGy-100kGy, and monitoring the irradiation dose rate in real time to ensure that the cross-linking of the material is fully completed.

Citation Information

Patent Citations

  • Phase change material-containing building heat-insulating coiled material and preparation method thereof

    CN110744897A

  • Phase-change thermal insulation composite material and preparation method thereof

    CN116355595A

  • Roof waterproof heat insulation coiled material and preparation method thereof

    CN117285885A

  • Urethane polyol prepolymer, porous polyurethane sheet and method of preparing the same

    US20050014858A1

Cited By

  • Polyurethane composition and composite material containing same

    CN119591827A