A lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy and a preparation method thereof
By adding Li and AlTiB to magnesium alloys, the body-centered cubic structure and the TiB2 dispersion strengthening phase are introduced, which solves the problem of difficulty in simultaneously improving the strength and plasticity of magnesium alloys and achieves the lightweight, high strength, toughness and good corrosion resistance of high-performance magnesium alloys. sex.
Patent Information
- Application Number
- CN202310293816.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-24
AI Technical Summary
Magnesium alloys tend to produce strong basal texture during plastic deformation, resulting in low strength and plasticity and poor corrosion resistance, making it difficult to achieve large-scale industrial application.
By adding Li to the magnesium alloy and controlling the amount of Li, a body-centered cubic structure is introduced, and AlTiB is added to generate a TiB2 dispersion strengthening phase, which refines the Mg matrix structure and improves the strength and toughness of the magnesium alloy while maintaining low density characteristics.
It significantly improves the plasticity, toughness and strength of Mg-Li-Al-TiB alloy, maintains its lightweight characteristics, and is suitable for industrial applications of high-performance magnesium alloys.
Smart Images

Figure CN116287917B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and in particular relates to a light-weight, high-strength and tough extruded Mg-Li-Al-TiB alloy and a preparation method thereof. Background Art
[0002] Magnesium alloys have the advantages of low density, high specific strength / specific stiffness, and excellent damping performance and biocompatibility. Therefore, magnesium alloys are widely used in aerospace, automotive industry, 3C electronics, biomedicine and other fields as a metal structural material. However, magnesium alloys are close-packed hexagonal metal structures, which easily produce strong basal textures during plastic deformation, resulting in low strength and plasticity, and easy deformation damage; while the low corrosion electrode potential and high corrosion current density of magnesium alloys make their corrosion resistance poor and easy to be corroded. Therefore, many shortcomings in the performance of magnesium alloys make it difficult to achieve large-scale industrial application. In the prior art, researchers usually use alloying and plastic processing methods to stimulate more non-basal slip in magnesium alloys by regulating texture, thereby simultaneously improving the strength and plasticity of magnesium alloys. At present, the development hotspot of high-performance magnesium alloys is to add Mg-Re alloys to the magnesium matrix, but the development cost of the rare earth element Re is too high, and the low density characteristics of magnesium alloys cannot be guaranteed after addition, and the performance of magnesium alloys cannot be effectively improved. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy in view of the deficiencies of the above-mentioned prior art. The alloy introduces a body-centered cubic structure into the alloy by adding Li and controlling the amount of Li added, thereby improving the plasticity and toughness of the Mg-Li-Al-TiB alloy, and generating a TiB2 dispersion strengthening phase belonging to the same Mg matrix crystal system by adding AlTiB, which has a good refinement effect on the Mg matrix structure, thereby significantly improving the strength and toughness of the Mg-Li-Al-TiB alloy, and maintaining a low density and lightweight characteristics, solving the problem that the strength and plasticity of magnesium alloys are difficult to improve simultaneously and the low-density characteristics cannot be guaranteed.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy, characterized in that it is made of the following components in mass percentage: Li 5.5% to 10%, Al 3.1% to 6.8%, AlTiB 0.1% to 3.7%, and the mass percentage of Al to AlTiB is 1.8:1 to 50:1, and the balance is Mg and unavoidable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 3.1% to 5.2%, B 0.8% to 3.2%, and the balance is Al and unavoidable impurity elements with a mass percentage of less than 0.1%; the density of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy is 1.45g / cm 3 ~1.52g / cm 3 , room temperature tensile strength is greater than 300MPa, room temperature yield strength is greater than 250MPa, and elongation is greater than 15%.
[0005] In the Mg-Li-Al-TiB alloy of the present invention, Li is added and the added mass percentage of Li is strictly controlled to be 5.5% to 10%, so that the hcp close-packed hexagonal crystal structure (α matrix) of the Mg matrix is partially transformed into a bcc body-centered cubic structure, that is, the plasticity and toughness of the Mg-Li-Al-TiB alloy are improved by introducing the body-centered cubic structure into the alloy; at the same time, the AlTiB added to the Mg-Li-Al-TiB alloy of the present invention reacts to generate TiB2 and Al3Ti in the melt after melting, and Al3Ti is quickly decomposed in the melt, while the dispersion strengthening phase T iB2 belongs to the hexagonal crystal system and the same crystal system as the α matrix. The interface energy between the two is small, which has a good refinement effect on the α matrix structure. Under the action of large-area non-uniform nucleation, the solidification structure of the Mg-Li-Al-TiB alloy is significantly refined, thereby significantly improving the mechanical properties. The added Al generates second phase particles in the alloy, further improving the mechanical properties of the alloy. In addition, by controlling the content ratio of each element in the Mg-Li-Al-TiB alloy of the present invention, the density of the Mg-Li-Al-TiB alloy is guaranteed to be low, thereby maintaining the lightweight characteristics.
[0006] The above-mentioned lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy is characterized in that it is made of the following components in mass percentage: Li 6.1% to 9.8%, Al 3.5% to 5.2%, AlTiB 0.1% to 1.6%, and the remainder is Mg and unavoidable impurity elements with a mass percentage of less than 0.15%.
[0007] The above-mentioned lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy is characterized in that it is made of the following components in mass percentage: Li 8%, Al 5%, AlTiB 1%, and the balance is Mg and inevitable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 5%, B 1%, and the balance is Al and inevitable impurity elements.
[0008] The above-mentioned lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy is characterized in that the crystal structure of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy is a close-packed hexagonal structure plus a body-centered cubic structure.
[0009] In addition, the present invention also provides a method for preparing the above-mentioned lightweight and high-strength extruded Mg-Li-Al-TiB alloy, characterized in that the method comprises the following steps:
[0010] Step 1, preheating: preheating Mg, Al, AlTiB master alloy; the preheating temperature is 210°C, the time is 20min, and air cooling;
[0011] Step 2, smelting: placing the preheated Mg, Al, and AlTiB master alloys in step 1 in a 1# smelting furnace at 700°C to 740°C under non-vacuum conditions for melting, placing Li in a 2# smelting furnace at 185°C to 200°C under non-vacuum conditions for melting, after all the materials in the 1# smelting furnace are melted into a melt, removing the scum and inserting an ultrasonic rod, using ultrasonic vibration to vibrate the melt for 2 minutes and then letting it stand for 5 minutes, then sending the Li liquid melted in the 2# smelting furnace into the 1# smelting furnace after ultrasonic vibration and standing under inert gas protection, and fully mixing with the melt to form an alloy melt;
[0012] Step 3, purification: after the temperature of the alloy melt in step 2 drops to 690°C to 700°C, add a refining agent, then heat to 720°C ± 3°C and keep warm for 3min to 10min for refining and purification, remove the scum and oscillate the purified alloy melt by ultrasonic for 2min to 5min and let it stand for 10min to 16min;
[0013] Step 4, casting: pouring the alloy melt after standing in step 3 into a water-cooled steel mold through a ceramic filter for rapid solidification to obtain an alloy ingot; the cooling rate of the rapid solidification is 150°C / s to 200°C / s;
[0014] Step 5, homogenization annealing: Wrap the alloy ingot obtained in step 4 with aluminum foil and place it in a precision CNC muffle furnace for homogenization annealing; the homogenization annealing temperature is 300°C ± 2°C, the holding time is 8h to 10h, and the furnace is cooled;
[0015] Step 6, slow extrusion: laying graphite paper along the inner wall of the extrusion cylinder, and then placing the alloy ingot after homogenization annealing in step 5 into the extrusion cylinder for extrusion deformation to obtain an extruded rod; the extrusion rate of the extrusion deformation is 4 mm / s to 10 mm / s, the extrusion temperature is 200° C. to 300° C., and the extrusion ratio is 15:1;
[0016] Step 7, medium-temperature solution treatment: subject the extruded rod obtained in step 6 to solution treatment to obtain a lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy; the solution treatment temperature is 250°C to 280°C, the insulation time is 20h to 35h, and the alloy is cooled in the furnace.
[0017] The present invention first preheats and removes water from the high-melting-point Mg, Al, and AlTiB master alloys in the raw materials and smelts them in the same smelting furnace to obtain a melt, and at the same time, smelts the low-melting-point Li in the raw materials separately to improve its yield, and then mixes the two and combines them with ultrasonic oscillation to form a uniform alloy melt, and then adds a high-density refining agent for refining and purification, removes silicon, iron, and nickel impurities in the alloy melt by adsorption, and then filters and removes impurities with a ceramic filter before casting the mold for rapid solidification, and combines with a water cooling device installed outside the steel mold to achieve rapid solidification so that the alloy ingot obtains a fine-grained structure; the present invention continues to The alloy ingot is subjected to homogenization annealing to eliminate the component segregation caused by local overcooling of the alloy ingot due to rapid solidification and improve the uniformity of the structure. Then, isothermal extrusion deformation is carried out to further eliminate local defects and promote the coordinated deformation of the internal slip deformation of the alloy ingot and the plastic strain between grains, which is beneficial for improving the strength and plasticity of the alloy. Then, medium-temperature solution treatment is performed to fully dissolve the dispersed strengthening phase AlLi generated during the solidification process into the matrix, so that the alloy is further strengthened after extrusion deformation, thereby obtaining a lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy.
[0018] The above method is characterized in that the inert gas in step 2 is a mixed gas of argon, nitrogen and sulfur hexafluoride.
[0019] The above method is characterized in that the refining agent in step 3 is composed of the following components in mass percentage: LiBr 36%, MgF 9%, CaF 9%, LiF 24%, LiCl 12%, and ZrCl4 10%. The refining agent composed of this component can effectively absorb impurities in the alloy melt, purify the alloy melt, and achieve a good refining effect.
[0020] The above method is characterized in that the frequency of the ultrasonic oscillation in step 2 and step 3 is 100 Hz. By controlling the frequency of the ultrasonic oscillation in the two-step process, the grains are refined to obtain an alloy ingot with a fine grain structure.
[0021] The above method is characterized in that the internal pore size of the ceramic filter in step 4 is 8 μm to 25 μm. By controlling the internal pore size of the ceramic filter, fine impurities and refining agents in the alloy melt are further removed to ensure that the alloy ingot obtains a fine grain structure.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] 1. In the Mg-Li-Al-TiB alloy of the present invention, Li is added and the amount of Li added is controlled to introduce a body-centered cubic structure into the alloy, thereby improving the plasticity and toughness of the Mg-Li-Al-TiB alloy. By adding AlTiB to generate a TiB2 dispersion strengthening phase belonging to the same Mg matrix crystal system, the Mg matrix structure is well refined, thereby significantly improving the strength and toughness of the Mg-Li-Al-TiB alloy, and the density is low, maintaining the lightweight characteristics.
[0024] 2. Compared with traditional AZ, ZK, rare earth magnesium alloys, the crystal structure of the Mg-Li-Al-TiB alloy of the present invention is a close-packed hexagonal structure plus a body-centered cubic structure, which has excellent plasticity while ensuring its lightness, and is conducive to subsequent plastic processing.
[0025] 3. Compared with rare earth magnesium alloys, the raw material costs of each component in the Mg-Li-Al-TiB alloy of the present invention are lower, which reduces the alloy development cost and is beneficial to the application of the alloy.
[0026] 4. The density of the Mg-Li-Al-TiB alloy of the present invention is 1.45 g / cm 3 ~1.52g / cm 3 , room temperature tensile strength greater than 300MPa, room temperature yield strength greater than 250MPa, elongation greater than 15%, suitable for pressure-bearing structural parts on bicycles.
[0027] 5. The preparation method of the present invention adopts constant temperature extrusion deformation combined with medium temperature solution treatment, which effectively eliminates local component segregation defects, promotes the coordinated deformation of internal slip deformation and plastic strain between grains of the alloy, and allows the dispersed strengthening phase AlLi to fully dissolve into the matrix to achieve strengthening, effectively improving the strength and plasticity of the Mg-Li-Al-TiB alloy.
[0028] 6. The preparation method of the present invention does not require vacuum conditions, has a short process flow, and is low in cost, which is conducive to the application and promotion of Mg-Li-Al-TiB alloy.
[0029] 7. The present invention controls the composition of the refining agent during the smelting process, effectively adsorbs impurities in the alloy melt, improves the purity of the alloy melt, and thus obtains a clean ingot without impurities.
[0030] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the solidification structure diagram of the alloy ingot prepared in Example 1 of the present invention.
[0032] Figure 2 This is the X-ray diffraction pattern of the alloy ingot prepared in Example 1 of the present invention.
[0033] Figure 3 This is the engineering stress-engineering strain curve of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy prepared in Example 1 of the present invention.
[0034] Figure 4 This is the solidification structure diagram of the alloy ingot prepared in Example 2 of the present invention.
[0035] Figure 5 This is the X-ray diffraction pattern of the alloy ingot prepared in Example 2 of the present invention.
[0036] Figure 6 This is the engineering stress-engineering strain curve of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy prepared in Example 2 of the present invention.
[0037] Figure 7 This is the solidification structure diagram of the alloy ingot prepared in Example 3 of the present invention.
[0038] Figure 8 This is the X-ray diffraction pattern of the alloy ingot prepared in Example 3 of the present invention.
[0039] Fig. 9 This is the engineering stress-engineering strain curve of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0040] Example 1
[0041] The lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy of this embodiment is made of the following components in mass percentage: Li 8.2%, Al 4.8%, AlTiB 0.1%, the balance being Mg and unavoidable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 5%, B 1%, the balance being Al and unavoidable impurity elements with a mass percentage of less than 0.1%.
[0042] The method for preparing the lightweight and high-strength extruded Mg-Li-Al-TiB alloy of this embodiment comprises the following steps:
[0043] Step 1, preheating: preheating Mg, Al, AlTiB master alloy; the preheating temperature is 210°C, the time is 20min, and air cooling;
[0044] Step 2, smelting: placing the preheated Mg, Al, and AlTiB master alloys in step 1 in a 1# smelting furnace at 740° C. and non-vacuum atmosphere conditions for melting, placing Li in a 2# smelting furnace at 200° C. and non-vacuum atmosphere conditions for melting, after all the materials in the 1# smelting furnace are melted into a melt, removing the scum and inserting an ultrasonic rod, using 100 Hz ultrasonic vibration to vibrate the melt for 2 minutes and then letting it stand for 5 minutes, then the Li liquid melted in the 2# smelting furnace is sent to the 1# smelting furnace after ultrasonic vibration and standing under the protection of inert gas, and fully mixed with the melt to form an alloy melt; the inert gas is a mixed gas composed of argon, nitrogen and sulfur hexafluoride in a volume ratio of 1:1:3;
[0045] Step 3, purification: after the temperature of the alloy melt in step 2 drops to 690°C-700°C, a refining agent is added, and then the temperature is raised to 720°C±3°C and kept warm for 3 minutes for refining and purification, after removing the scum, the alloy melt is purified by 100Hz ultrasonic vibration for 2 minutes and allowed to stand for 12 minutes; the refining agent is composed of the following components by mass percentage: LiBr 36%, MgF 9%, CaF 9%, LiF 24%, LiCl 12%, ZrCl4 10%;
[0046] Step 4, casting: pouring the alloy melt after standing in step 3 into a water-cooled steel mold through a ceramic filter with an internal pore size of 8 μm to 25 μm for rapid solidification to obtain an alloy ingot; the cooling rate of the rapid solidification is 200°C / s;
[0047] Step 5, homogenization annealing: Wrap the alloy ingot obtained in step 4 with aluminum foil and place it in a precision CNC muffle furnace for homogenization annealing; the homogenization annealing temperature is 300°C ± 2°C, the holding time is 10h, and the furnace is cooled;
[0048] Step 6, slow extrusion: laying graphite paper along the inner wall of the extrusion barrel, and then cutting and grinding the alloy ingot after homogenization annealing in step 5 until the surface is smooth, and then putting it into the extrusion barrel for extrusion deformation to obtain an extruded rod; the extrusion rate of the extrusion deformation is 6 mm / s, the extrusion temperature is 300°C ± 5°C, and the extrusion ratio is 15:1;
[0049] Step 7: Medium temperature solid solution: The extruded rod obtained in step 6 is placed in a muffle furnace for solid solution treatment to obtain a density of 1.47 g / cm 3 Lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy; the solution treatment temperature is 280°C, the holding time is 20 hours, and the furnace is cooled.
[0050] Figure 1 is the solidification structure diagram of the alloy ingot prepared in this embodiment, Figure 2 The X-ray diffraction pattern of the alloy ingot prepared in this embodiment is shown in FIG. Figure 1 and Figure 2 It can be seen that the crystal structure of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy is a close-packed hexagonal structure plus a body-centered cubic structure.
[0051] Figure 3 The engineering stress-engineering strain curve of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy prepared in this embodiment is shown in Figure 2. Figure 3 It can be seen that the room temperature tensile strength of the lightweight and high-strength extruded Mg-Li-Al-TiB alloy is 310.8 MPa, the room temperature yield strength is 264.8 MPa, and the elongation is 21.5%.
[0052] Example 2
[0053] The high-quality, high-strength and tough extruded Mg-Li-Al-TiB alloy of this embodiment is composed of the following components in mass percentage: Li 7.5%, Al 5.8%, AlTiB 0.5%, the balance is Mg and unavoidable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 5%, B 1%, the balance is Al and unavoidable impurity elements with a mass percentage of less than 0.1%.
[0054] The difference between the preparation method of high-quality and tough extruded Mg-Li-Al-TiB alloy in this embodiment and the preparation method in Example 1 is that the temperature of the solution treatment in step 7 is 265°C, the holding time is 30h, and the density is 1.50g / cm 3 β-phase high-strength Mg-Li-Al-TiB alloy.
[0055] Figure 4 is the solidification structure diagram of the alloy ingot prepared in this embodiment, Figure 5 The X-ray diffraction pattern of the alloy ingot prepared in this embodiment is shown in FIG. Figure 4 and Figure 5 It can be seen that the crystal structure of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy is a close-packed hexagonal structure plus a body-centered cubic structure.
[0056] Figure 6 The engineering stress-engineering strain curve of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy prepared in this embodiment is shown in Figure 2. Figure 6It can be seen that the room temperature tensile strength of the lightweight and high-strength extruded Mg-Li-Al-TiB alloy is 311.3 MPa, the room temperature yield strength is 259.8 MPa, and the elongation is 17.7%.
[0057] Example 3
[0058] The high-quality, high-strength and tough extruded Mg-Li-Al-TiB alloy of this embodiment is composed of the following components in mass percentage: Li 9.3%, Al 6.2%, AlTiB 1.2%, the balance is Mg and unavoidable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 5%, B 1%, the balance is Al and unavoidable impurity elements with a mass percentage of less than 0.1%.
[0059] The difference between the preparation method of high-quality and tough extruded Mg-Li-Al-TiB alloy in this embodiment and the preparation method in Example 1 is that the temperature of the solid solution treatment in step 7 is 270°C, the holding time is 24h, and the density is 1.45g / cm 3 β-phase high-strength Mg-Li-Al-TiB alloy.
[0060] Figure 7 is the solidification structure diagram of the alloy ingot prepared in this embodiment, Figure 8 The X-ray diffraction pattern of the alloy ingot prepared in this embodiment is shown in FIG. Figure 7 and Figure 8 It can be seen that the crystal structure of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy is a close-packed hexagonal structure plus a body-centered cubic structure.
[0061] Fig. 9 The engineering stress-engineering strain curve of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy prepared in this embodiment is shown in Figure 2. Fig. 9 It can be seen that the room temperature tensile strength of the lightweight and high-strength extruded Mg-Li-Al-TiB alloy is 321.3 MPa, the room temperature yield strength is 262.3 MPa, and the elongation is 17.1%.
[0062] Example 4
[0063] The lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy of this embodiment is made of the following components in mass percentage: Li 8%, Al 5%, AlTiB 1%, the balance being Mg and unavoidable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 5%, B 1%, the balance being Al and unavoidable impurity elements with a mass percentage of less than 0.1%.
[0064] The method for preparing the lightweight and high-strength extruded Mg-Li-Al-TiB alloy of this embodiment comprises the following steps:
[0065] Step 1, preheating: preheating Mg, Al, AlTiB master alloy; the preheating temperature is 210°C, the time is 20min, and air cooling;
[0066] Step 2, smelting: placing the preheated Mg, Al, and AlTiB master alloys in step 1 in a 1# smelting furnace at 720° C. and non-vacuum atmosphere conditions for melting, placing Li in a 2# smelting furnace at 200° C. and non-vacuum atmosphere conditions for melting, after all the materials in the 1# smelting furnace are melted into a melt, removing the scum and inserting an ultrasonic rod, using 100 Hz ultrasonic vibration to vibrate the melt for 2 minutes and then letting it stand for 5 minutes, then sending the Li liquid melted in the 2# smelting furnace into the 1# smelting furnace after ultrasonic vibration and standing under the protection of inert gas, and fully mixing with the melt to form an alloy melt; the inert gas is a mixed gas composed of argon, nitrogen and sulfur hexafluoride in a volume ratio of 1:1:3;
[0067] Step 3, purification: after the temperature of the alloy melt in step 2 drops to 690°C-700°C, a refining agent is added, and then the temperature is raised to 720°C±3°C and kept warm for 5 minutes for refining and purification, after removing the scum, the alloy melt is purified by 100Hz ultrasonic vibration for 3 minutes and allowed to stand for 12 minutes; the refining agent is composed of the following components in mass percentage: LiBr 36%, MgF 9%, CaF 9%, LiF 24%, LiCl 12%, ZrCl4 10%;
[0068] Step 4, casting: pouring the alloy melt after standing in step 3 into a water-cooled steel mold through a ceramic filter with an internal pore size of 8 μm to 25 μm for rapid solidification to obtain an alloy ingot; the cooling rate of the rapid solidification is 180°C / s;
[0069] Step 5, homogenization annealing: Wrap the alloy ingot obtained in step 4 with aluminum foil and place it in a precision CNC muffle furnace for homogenization annealing; the homogenization annealing temperature is 300°C ± 2°C, the holding time is 9h, and the furnace is cooled;
[0070] Step 6, slow extrusion: laying graphite paper along the inner wall of the extrusion cylinder, and then cutting and grinding the alloy ingot after homogenization annealing in step 5 until the surface is smooth, and then putting it into the extrusion cylinder for extrusion deformation to obtain an extruded rod; the extrusion rate of the extrusion deformation is 8 mm / s, the extrusion temperature is 280°C ± 5°C, and the extrusion ratio is 15:1;
[0071] Step 7: Medium temperature solid solution: The extruded rod obtained in step 6 is placed in a muffle furnace for solid solution treatment to obtain a density of 1.47 g / cm3 Lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy; the solution treatment temperature is 260°C, the holding time is 30 hours, and the furnace is cooled.
[0072] After testing, the room temperature tensile strength of the lightweight and high-strength extruded Mg-Li-Al-TiB alloy is 329.1 MPa, the room temperature yield strength is 267.5 MPa, and the elongation is 22.3%.
[0073] Example 5
[0074] The high-quality, high-strength and tough extruded Mg-Li-Al-TiB alloy of this embodiment is composed of the following components in mass percentage: Li 10%, Al 3.1%, AlTiB 1%, the balance being Mg and unavoidable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 3.1%, B 0.8%, the balance being Al and unavoidable impurity elements with a mass percentage of less than 0.1%.
[0075] The method for preparing the lightweight and high-strength extruded Mg-Li-Al-TiB alloy of this embodiment comprises the following steps:
[0076] Step 1, preheating: preheating Mg, Al, AlTiB master alloy; the preheating temperature is 210°C, the time is 20min, and air cooling;
[0077] Step 2, smelting: placing the preheated Mg, Al, and AlTiB master alloys in step 1 in a 1# smelting furnace at 700° C. and non-vacuum atmosphere conditions for melting, placing Li in a 2# smelting furnace at 185° C. and non-vacuum atmosphere conditions for melting, after all the materials in the 1# smelting furnace are melted into a melt, removing the scum and inserting an ultrasonic rod, oscillating the melt with 100 Hz ultrasound for 2 minutes and then letting it stand for 5 minutes, then sending the Li liquid melted in the 2# smelting furnace into the 1# smelting furnace after ultrasonic oscillation and standing under the protection of inert gas, and fully mixing with the melt to form an alloy melt; the inert gas is a mixed gas composed of argon, nitrogen and sulfur hexafluoride in a volume ratio of 1:1:3;
[0078] Step 3, purification: after the temperature of the alloy melt in step 2 drops to 690°C-700°C, a refining agent is added, and then the temperature is raised to 720°C±3°C and kept warm for 10 minutes for refining and purification, after removing the scum, the alloy melt is purified by 100Hz ultrasonic vibration for 5 minutes and then left to stand for 16 minutes; the refining agent is composed of the following components in mass percentage: LiBr 36%, MgF 9%, CaF 9%, LiF 24%, LiCl 12%, ZrCl4 10%;
[0079] Step 4, casting: pouring the alloy melt after standing in step 3 into a water-cooled steel mold through a ceramic filter with an internal pore size of 8 μm to 25 μm for rapid solidification to obtain an alloy ingot; the cooling rate of the rapid solidification is 150°C / s;
[0080] Step 5, homogenization annealing: Wrap the alloy ingot obtained in step 4 with aluminum foil and place it in a precision CNC muffle furnace for homogenization annealing; the homogenization annealing temperature is 300°C ± 2°C, the holding time is 8h, and the furnace is cooled;
[0081] Step 6, slow extrusion: laying graphite paper along the inner wall of the extrusion cylinder, and then cutting and grinding the alloy ingot after homogenization annealing in step 5 until the surface is smooth, and then putting it into the extrusion cylinder for extrusion deformation to obtain an extruded rod; the extrusion rate of the extrusion deformation is 4 mm / s, the extrusion temperature is 250°C ± 5°C, and the extrusion ratio is 15:1;
[0082] Step 7: Medium temperature solution treatment: The extruded rod obtained in step 6 is placed in a muffle furnace for solution treatment to obtain a density of 1.45 g / cm 3 Lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy; the solution treatment temperature is 260°C, the holding time is 35h, and the furnace is cooled.
[0083] After testing, the room temperature tensile strength of the lightweight and high-strength extruded Mg-Li-Al-TiB alloy is 305.5MPa, the room temperature yield strength is 254.1MPa, and the elongation is 23.7%.
[0084] Example 6
[0085] The high-quality, high-strength and tough extruded Mg-Li-Al-TiB alloy of this embodiment is composed of the following components in mass percentage: Li 5.5%, Al 6.8%, AlTiB 3.7%, the balance is Mg and unavoidable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 5.2%, B 3.2%, the balance is Al and unavoidable impurity elements with a mass percentage of less than 0.1%.
[0086] The difference between the preparation method of high-quality and tough extruded Mg-Li-Al-TiB alloy in this embodiment and the preparation method in Example 4 is that the standing time in step 3 is 10 min; the extrusion rate of extrusion deformation in step 6 is 10 mm / s; the extrusion temperature in step 6 is 200°C ± 5°C; the temperature of solution treatment in step 7 is 250°C, and the density is 1.52 g / cm 3 β-phase high-strength Mg-Li-Al-TiB alloy.
[0087] After testing, the room temperature tensile strength of the lightweight and high-strength extruded Mg-Li-Al-TiB alloy is 331.1 MPa, the room temperature yield strength is 270.4 MPa, and the elongation is 18.9%.
[0088] Example 7
[0089] The high-quality, high-strength and tough extruded Mg-Li-Al-TiB alloy of this embodiment is composed of the following components in mass percentage: Li 6.1%, Al 5.2%, AlTiB 1.6%, the balance is Mg and unavoidable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 5%, B 1%, the balance is Al and unavoidable impurity elements with a mass percentage of less than 0.1%.
[0090] The difference between the method for preparing high-quality and tough extruded Mg-Li-Al-TiB alloy in this embodiment and the method for preparing in Example 4 is that the extrusion temperature in step 6 is 240°C ± 5°C; the density obtained in step 7 is 1.50 g / cm 3 β-phase high-strength Mg-Li-Al-TiB alloy.
[0091] After testing, the room temperature tensile strength of the lightweight and high-strength extruded Mg-Li-Al-TiB alloy is 324.5MPa, the room temperature yield strength is 266.0MPa, and the elongation is 20.3%.
[0092] Example 8
[0093] The high-quality, high-strength and tough extruded Mg-Li-Al-TiB alloy of this embodiment is composed of the following components in mass percentage: Li 9.8%, Al 3.5%, AlTiB 0.2%, the balance being Mg and unavoidable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 5%, B 1%, the balance being Al and unavoidable impurity elements with a mass percentage of less than 0.1%.
[0094] The difference between the preparation method of high-quality and tough extruded Mg-Li-Al-TiB alloy in this embodiment and the preparation method in Example 4 is that the extrusion temperature in step 6 is 250°C ± 5°C; the density obtained in step 7 is 1.46 g / cm 3 β-phase high-strength Mg-Li-Al-TiB alloy.
[0095] After testing, the room temperature tensile strength of the lightweight and high-strength extruded Mg-Li-Al-TiB alloy is 306.3MPa, the room temperature yield strength is 258.9MPa, and the elongation is 22.1%.
[0096] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy, characterized in that: The alloy is made of the following components in mass percentage: Li 5.5%-10%, Al 3.1%-6.8%, AlTiB 0.1%-3.7%, and the mass percentage of Al to AlTiB is 1.8:1-50:1, and the balance is Mg and unavoidable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 3.1%-5.2%, B 0.8%-3.2%, and the balance is Al and unavoidable impurity elements with a mass percentage of less than 0.1%; the density of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy is 1.45g / cm 3 ~1.52g / cm 3 , room temperature tensile strength greater than 300MPa, room temperature yield strength greater than 250MPa, and elongation greater than 15%; the crystal structure of the lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy is a close-packed hexagonal structure plus a body-centered cubic structure; The preparation method of the lightweight and high-strength extruded Mg-Li-Al-TiB alloy comprises the following steps: Step 1, preheating: preheating Mg, Al, AlTiB master alloy; the preheating temperature is 210°C, the time is 20min, and air cooling; Step 2, smelting: placing the preheated Mg, Al, and AlTiB master alloys in step 1 in a 1# smelting furnace at 700°C-740°C and non-vacuum conditions for melting, placing Li in a 2# smelting furnace at 185°C-200°C and non-vacuum conditions for melting, after all the materials in the 1# smelting furnace are melted into a melt, removing the scum and inserting an ultrasonic rod, using ultrasonic vibration to vibrate the melt for 2 minutes and then letting it stand for 5 minutes, then sending the Li liquid melted in the 2# smelting furnace into the 1# smelting furnace after ultrasonic vibration and standing under the protection of inert gas, and fully mixing with the melt to form an alloy melt; Step 3, purification: After the temperature of the alloy melt in step 2 drops to 690°C~700°C, add a refining agent, then heat it to 720°C±3°C and keep it warm for 3min~10min for refining and purification, remove the scum and use ultrasonic vibration to purify the alloy melt for 2min~5min and let it stand for 10min~16min; Step 4, casting: pouring the alloy melt after standing in step 3 into a water-cooled steel mold through a ceramic filter for rapid solidification to obtain an alloy ingot; the cooling rate of the rapid solidification is 150°C / s to 200°C / s; Step 5, homogenization annealing: Wrap the alloy ingot obtained in step 4 with aluminum foil and place it in a precision CNC muffle furnace for homogenization annealing; the homogenization annealing temperature is 300°C ± 2°C, the holding time is 8h~10h, and the furnace is cooled; Step 6, slow extrusion: laying graphite paper along the inner wall of the extrusion barrel, and then placing the alloy ingot after homogenization annealing in step 5 into the extrusion barrel for extrusion deformation to obtain an extruded rod; the extrusion rate of the extrusion deformation is 4 mm / s~10 mm / s, the extrusion temperature is 200°C~300°C, and the extrusion ratio is 15:1; Step 7, medium-temperature solution treatment: subject the extruded rod obtained in step 6 to solution treatment to obtain a lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy; the solution treatment temperature is 250°C to 280°C, the insulation time is 20h to 35h, and the alloy is cooled with the furnace.
2. A lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy according to claim 1, characterized in that: It is made of the following components in mass percentage: Li 6.1%~9.8%, Al 3.5%~5.2%, AlTiB 0.1%~1.6%, and the balance is Mg and unavoidable impurity elements with a mass percentage of less than 0.15%.
3. A lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy according to claim 1, characterized in that: It is made of the following components in mass percentage: Li 8%, Al 5%, AlTiB 1%, and the balance is Mg and inevitable impurity elements with a mass percentage of less than 0.15%; the AlTiB is composed of the following components in mass percentage: Ti 5%, B 1%, and the balance is Al and inevitable impurity elements.
4. A lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy according to claim 1, characterized in that: The inert gas in step 2 is a mixed gas of argon, nitrogen and sulfur hexafluoride.
5. A lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy according to claim 1, characterized in that: The refining agent in step 3 is composed of the following components in percentage by weight: Composition: LiBr 36%, MgF 9%, CaF 9%, LiF 24%, LiCl 12%, ZrCl4 10%.
6. A lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy according to claim 1, characterized in that: The frequency of the ultrasonic oscillation in step 2 and step 3 is 100 Hz.
7. A lightweight, high-strength and tough extruded Mg-Li-Al-TiB alloy according to claim 1, characterized in that: The internal pore size of the ceramic filter in step 4 is 8 μm to 25 μm.
Citation Information
Patent Citations
Method for refining LA141 magnesium-lithium alloy grains
CN101713034A
Mg-Li-Si alloy and preparation method thereof
CN104046869A
Method for preparing high-strength magnesium-lithium alloy by quick setting by using copper mold and copper mold
CN104946947A
High-strength ultra-light two-phase structure magnesium-lithium alloy plate and preparation method thereof
CN106834843A
High-strength low-density hcp+bcc dual-structure magnesium-lithium alloy bar and preparation method thereof
CN108179335A