A method for preparing metal aerogel in-situ grown carbon nanotubes
By growing carbon nanotubes in situ in the 3D structure of metal aerogels, forming a three-dimensional macroscopic and self-supporting network structure, the problem of the failure to fully realize the application potential of metal aerogels in the field of electrocatalysis and achieving efficient electron transmission and unique properties reduce costs.
Patent Information
- Application Number
- CN202310277905.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There is currently no technology to control the growth of carbon nanotubes in situ by metal aerogels, which limits the application potential of metal aerogels in fields such as electrocatalysis.
Using the combination of sol-gel method and supercritical drying/freeze-drying, the metal aerogel is achieved in situ growth of carbon nanotubes in the 3D structure of metal aerogel by changing external conditions such as magnetic field, temperature and gas phase treatment. The preparation of metal aerogel-carbon nanotubes forms a three-dimensional macroscopic, self-supporting network structure.
The preparation of metal aerogel in situ grown carbon nanotubes is realized, giving the product rich active sites, efficient electron transport channels and unique optical and electrical properties, with excellent electrocatalytic properties, and reducing the cost of the finished product. .
Smart Images

Figure CN116288241B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material preparation, and in particular relates to a method for preparing metal aerogel in-situ grown carbon nanotubes. Background Art
[0002] Aerogel is known as one of the "10 magical materials that changed the world" due to its extremely low density, extremely small pore size, extremely low thermal insulation coefficient, and extremely low sound propagation speed. It has set 15 "Guinness World Records". Aerogel is the world's smallest solid and one of the top ten emerging technologies in the field of chemistry in 2022.
[0003] The current mainstream aerogel preparation process is a combination of sol-gel method and supercritical drying. Different compounds form various aerogels through the aerogel preparation process, enriching the variety of aerogels. Among them, the most common and most mature aerogel is silica aerogel, which belongs to oxide aerogel. In addition, there are carbide aerogel, nitride aerogel, metal aerogel, organic aerogel, carbon aerogel, biomass aerogel, composite aerogel and other aerogels.
[0004] Among them, metal aerogel is a gel constructed entirely of metal nanostructures. It only emerged about 10 years ago, and the corresponding aerogel research is still in its infancy. It combines the properties of metals (conductivity, catalytic activity, etc.) and the advantages of gels (self-supporting structure, porous network and large specific surface area, etc.). Given its 3D conductive path, numerous isolated and highly active catalytic sites and unusual plasma properties, metal aerogel has shown incredible application potential, especially in electrocatalysis.
[0005] Carbon nanotubes are one-dimensional cylindrical hollow structures, which can also be understood as rolled graphite sheets, with a diameter of nanometers and a length of micrometers. 2 The unique one-dimensional nanostructure constructed by hybrid carbon atoms endows carbon nanotubes with excellent physical, chemical and structural properties, such as large specific surface area (theoretical surface area up to 1315 m 2 / g), excellent mechanical strength (the Young's modulus of a single single-walled carbon nanotube can reach 1 TPa) and high electrical conductivity (more than 1×10 5 S / m), chemical stability, controllable porous structure, etc.
[0006] This project uses metal aerogels to control the in-situ growth of carbon nanotubes. By growing carbon nanotubes on the surface of metal aerogels and between their pores, a three-dimensional macroscopic, self-supporting network structure of metal aerogel-carbon nanotubes is obtained, which has abundant active sites, efficient electron transport channels, and unique optical and electrical properties. At present, no metal aerogels have been reported to control the in-situ growth of carbon nanotubes. Summary of the invention
[0007] The purpose of the present invention is to provide a method for preparing metal aerogel in-situ grown carbon nanotubes, so as to fill the gap in the current technology of metal aerogel in-situ controlled growth of carbon nanotubes; metal aerogel is used as a framework and catalyst to control the growth of carbon nanotubes in its 3D structure to form a three-dimensional macroscopic, self-supporting network structure of metal aerogel-carbon nanotubes.
[0008] To achieve the above object, the present invention adopts the following technical solution: a method for preparing carbon nanotubes by in-situ growth of metal aerogel, comprising the following steps:
[0009] Step 1: introducing a metal solution, a solvent, a ligand solution, a reducing agent, and an initiator into a reaction vessel, and then self-assembling the metal hydrogel by changing external conditions, such as a magnetic field, temperature, etc., washing the metal hydrogel multiple times, exchanging the metal hydrogel with an alcohol solution, and freeze-drying the metal aerogel; wherein the freeze-drying temperature is 0-77 K;
[0010] Step 2: Place the obtained metal aerogel into a reaction chamber, and heat the reaction chamber to 300°C-1500°C under inert gas protection, and keep the temperature for 30 min-60 min;
[0011] Step 3, continuously introducing reducing gas, inert gas and gaseous carbon-containing organic matter into the reaction chamber, and continuously reacting to obtain a composite material of metal aerogel in-situ grown carbon nanotubes;
[0012] The ratio of reducing gas, inert gas and gaseous carbon-containing organic matter is 0.1-10:1:0.01-50.
[0013] Furthermore, the metal solution in step one is a mixture of one or more metal solutions of aluminum, magnesium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, gallium, zirconium, molybdenum, ruthenium, rhodium, palladium, silver, tin, gold, and platinum in any proportion.
[0014] Furthermore, in step 1, the physical properties of the metal aerogel are adjusted by changing the pressure; the pressure in step 1 ranges from 1Pa to 100MPa.
[0015] Furthermore, in step 1, the physical properties of the metal aerogel include shape, density, pores and spacing.
[0016] Furthermore, in step 2, the heating rate of the reaction chamber is 3°C / min-40°C / min.
[0017] Furthermore, the inert gas in step 2 is one or more of nitrogen, argon or helium.
[0018] Furthermore, the reaction chamber in step 2 is a vertical tube furnace or a horizontal tube furnace.
[0019] Furthermore, the inert gas in step three is one or more of nitrogen, argon or helium; the gaseous carbon-containing organic matter is a carbon-containing organic gas or a vaporized organic liquid, and the vaporization temperature of the organic liquid is 100°C-300°C.
[0020] Furthermore, in step three, the carbon-containing organic gas is a mixture of one or more of methane, natural gas, ethane, ethylene, acetylene, propane, and propylene; and the gasified organic liquid is a mixture of one or more of anhydrous methanol, anhydrous ethanol, benzene, toluene, and xylene.
[0021] Furthermore, the composite material in step three utilizes metal aerogel as a framework and catalyst to control the growth of carbon nanotubes in its 3D structure, thereby forming a three-dimensional macroscopic, self-supporting network structure of metal aerogel-carbon nanotubes.
[0022] The structure has abundant active sites, efficient electron transport channels, and unique optical and electrical properties.
[0023] Furthermore, the continuous reaction time in step three is 1 min-60 min.
[0024] The beneficial effects of the present invention are embodied in:
[0025] 1. The present invention provides a method for preparing carbon nanotubes grown in situ by metal aerogel, which realizes the in situ controlled growth of carbon nanotubes by metal aerogel for the first time by combining sol-gel, supercritical drying / freeze drying and chemical vapor deposition.
[0026] 2. The present invention provides a method for preparing carbon nanotubes by in-situ growth of metal aerogels. The metal aerogels act as a framework and catalyst to control the growth of carbon nanotubes in their 3D structure, forming a three-dimensional macroscopic, self-supporting network structure of metal aerogel-carbon nanotubes. The structure has abundant active sites, efficient electron transmission channels, and unique optical and electrical properties.
[0027] 3. The product obtained by the present invention protects the excellent properties of the metal aerogel as much as possible, while growing a large number of carbon nanotubes on its surface, and is expected to become a composite material with excellent electrocatalytic performance.
[0028] 4. The present invention can use active metals to perfectly replace precious metals, effectively reducing the cost of finished products.
[0029] Other features and advantages of the present invention will be described in the following description, and partly become obvious from the description, or be understood by practicing the present invention. The main purpose and other advantages of the present invention can be realized and obtained by the schemes particularly pointed out in the description. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The present invention will be further described in detail below in conjunction with the accompanying drawings.
[0031] Figure 1 This is an optical photograph of the metal aerogel of the present invention.
[0032] Figure 2 are SEM and TEM images of different metal aerogels.
[0033] Figure 3 These are optical photographs of the metal aerogel after being pressed at 53 KPa (top view and side view).
[0034] Figure 4 This is a TEM image of carbon nanotubes after in-situ growth of metal aerogel.
[0035] Figure 5 This is a schematic diagram of the microstructure of in-situ grown carbon nanotubes in metal aerogel.
[0036] Figure 6 This is a SEM image of the metal aerogel after in-situ growth of carbon nanotubes in implementation case 1.
[0037] Figure 7 It is the OER performance diagram after the growth of Fe aerogels with different weights.
[0038] Figure 8 This is a SEM image of the metal aerogel after in-situ growth of carbon nanotubes in implementation case 2.
[0039] Fig. 9 This is the SEM image of the metal aerogel after in-situ growth of carbon nanotubes in implementation case three. Implementation
[0040] The technical solution of the present invention is described in detail below through examples. The following examples are merely exemplary and can only be used to explain and illustrate the technical solution of the present invention, but cannot be interpreted as limiting the technical solution of the present invention.
[0041] The object of the present invention is to provide a method for preparing carbon nanotubes grown in situ by metal aerogel, comprising the following steps:
[0042] Step 1: introduce metal solution, solvent, ligand solution, reducing agent and initiator into a reaction vessel, and then self-assemble to form metal hydrogel by changing external conditions, i.e., sol-gel method, wash several times, exchange with alcohol solution and freeze-dry to obtain metal aerogel; the metal solution in step 1 is one or more metal solutions of aluminum, magnesium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, gallium, zirconium, molybdenum, ruthenium, rhodium, palladium, silver, tin, gold and platinum mixed in any ratio. Step 1: adjust the physical properties of metal aerogel by changing the pressure; the pressure range of the pressure in step 1 is 100 Pa-100 MPa. The physical properties of metal aerogel in step 1 include shape, density, pores and spacing.
[0043] Step 2: Place the obtained metal aerogel into a reaction chamber, and heat the reaction chamber to 300°C-1500°C under inert gas protection, and keep warm for 30 min-60 min; the heating rate of the reaction chamber in step 2 is 3°C / min-40°C / min. The inert gas in step 2 is one or more of nitrogen, argon or helium. The reaction chamber in step 2 is a vertical tube furnace or a horizontal tube furnace.
[0044] Step three, continuously introducing reducing gas, inert gas and gaseous carbon-containing organic matter into the reaction chamber, and continuously reacting to obtain a composite material of metal aerogel in-situ grown carbon nanotubes.
[0045] The inert gas in step three is one or more of nitrogen, argon or helium; the gaseous carbon-containing organic matter is a carbon-containing organic gas or a vaporized organic liquid, and the vaporization temperature of the organic liquid is 100°C-300°C. The continuous reaction time in step three is 1 min-60 min. In step three, the carbon-containing organic gas is a mixture of one or more of methane, natural gas, ethane, ethylene, acetylene, propane, and propylene; the vaporized organic liquid is a mixture of one or more of anhydrous methanol, anhydrous ethanol, benzene, toluene, and xylene. The composite material in step three uses metal aerogel as a framework and catalyst to control the growth of carbon nanotubes in its 3D structure to form a three-dimensional macroscopic, self-supporting network structure of metal aerogel-carbon nanotubes.
[0046] Figure 1 is an optical photograph of the metal aerogel of the present invention. Figure 1 A macroscopic optical photograph of metal aerogel can be seen in. Figure 2 are SEM and TEM images of different metal aerogels. Figure 3 , Figure 4 These are optical photographs of the metal aerogel after being pressed at 53 KPa (top view and side view). Figure 5This is a schematic diagram of the microstructure of in-situ grown carbon nanotubes on aerometal. It can be seen that the in-situ grown carbon nanotubes should be distributed on the surface of the aerometal, and the carbon nanotubes themselves are arranged in a disordered manner. The structure provided by the present invention has abundant active sites, efficient electron transmission channels, and unique optical and electrical properties.
[0047] From above Figure 6 It can be seen that the composite structure of carbon nanotubes and metal aerogels is an aerogel structure that ensures the growth of carbon nanotubes. Since the size of the metal aerogels we prepared is tens of nanometers, the aerogels will change from solid to liquid due to the size effect under the high temperature of CVD, so the size will increase to a certain extent, or even collapse. The three-dimensional macroscopic, self-supporting network structure should be considered the basic characteristics of aerogels. Example
[0048] 1. First, take 10 ml of the prepared 188 mM (NH4)2RuCl6 aqueous solution and add it to 100 ml of deionized water. After stirring and dispersing it evenly with a magnetic stirrer, add 3 ml of 1 M NaBH4 solution. The solution quickly turns black. After removing the magnetic stirrer and standing for 2-8 hours, the black gel will settle at the bottom of the container or float on the solution. The obtained gel is purified 6-8 times with a large amount of deionized water, and the total purification time is 2-3 days. Then, the gel is solvent exchanged with tert-butanol at 303 K for 3-4 times, and the exchange time is 2 days. After that, the gel is quickly frozen with liquid nitrogen and kept at 77 K for about 10-15 min. Finally, the frozen sample is freeze-dried at about 1Pa and -80°C for 12-24 h to obtain Ru aerogel.
[0049] 2. Place the ruthenium metal aerogel in a quartz boat and place it in the reaction chamber. Heat the reaction chamber to 660°C at a heating rate of 5°C / min under N2 protection and keep it warm for 45 minutes.
[0050] 3. A mixed gas of N2, H2 and C3H6 was continuously introduced into the reaction chamber for 0.25 h to obtain a black solid; the flow ratio of N2, H2 and C3H6 in the mixed gas was 3:4:1. The SEM image of the obtained ruthenium aerogel in situ grown carbon nanotubes is shown in Figure 6 As shown in FIG. 1 , both the aerogel and the carbon nanotubes mentioned above exist and are perfectly combined together. Example
[0051] 1. First, take 10 ml of the prepared 325 mM FeCl3 aqueous solution and add it to 100 ml of deionized water. After stirring and dispersing it evenly with a magnetic stirrer, add 4 ml of 1 M NaBH4 solution and 10 ml of 10 M NH4F solution in sequence. The solution quickly turns black. After removing the magnetic stirrer and standing for 2-8 hours, the black gel will settle at the bottom of the container or float on the solution. The obtained gel is purified 6-8 times with a large amount of deionized water, and the total purification time is 2-3 days. Then, the gel is solvent exchanged with tert-butanol at 303 K for 3-4 times, and the exchange time is 2 days. After that, the gel is quickly frozen with liquid nitrogen and kept at 77 K for about 10-15 min. Finally, the frozen sample is freeze-dried at about 1 Pa and -80 ° C for 12-24 hours to obtain Fe aerogel.
[0052] 2. Place the Fe metal aerogel in a quartz boat and place it in the reaction chamber. Heat the reaction chamber to 710°C at a heating rate of 5°C / min under Ar protection and keep it warm for 35 min.
[0053] 3. Continue to introduce a mixed gas of Ar, H2 and C3H8 into the reaction chamber for 35 min to obtain a black solid, which is a composite material of iron aerogel in situ grown carbon nanotubes; the flow ratio of Ar, H2 and C3H8 in the mixed gas is 1.5:2:1. The SEM image of the obtained aerogel in situ grown carbon nanotubes is shown in Figure 7 shown. Figure 8 , Fig. 9 The figures are on the same scale.
[0054] As shown in the figure, Fe metal aerogel (20 mM) was prepared under the same conditions by the sol-gel method, and then different g of Fe aerogel were weighed, namely 0.5 g, 1 g, 1.5 g, 2 g, and 2.5 g (refer to Figure 7 ), and then pressed (pressing conditions 53kPa), and then grew under the same conditions using chemical vapor deposition. Finally, the OER performance of the grown metal aerogel-carbon nanotube composite material was characterized and compared with commercial Ir / C. It was found that under the regulation of our method, the overpotential of the prepared sample could be close to or even exceed that of commercial one. Example
[0055] First, take 10 ml of the prepared 325 mM (NH4)2RuCl6 and NiCl2 aqueous solutions and add them to 100 ml of deionized water in turn. After being dispersed evenly with a magnetic stirrer, add 40 ml of 0.5 M NaBH4 solution and 10 ml of 10 M NH4F solution in turn. The solution quickly turns black. After removing the magnetic stirrer and standing for 2-8 hours, the black gel will be deposited at the bottom of the container or float on the solution. The obtained gel is purified 6-8 times with a large amount of deionized water, and the total purification time is 2-3 days. Then, the gel is solvent exchanged with tert-butanol at 303 K for 3-4 times, and the exchange time is 2 days. After that, the gel is quickly frozen with liquid nitrogen and kept at 77 K for about 10-15 min. Finally, the frozen sample is freeze-dried at about 1 Pa and -80 ° C for 12-24 h to obtain ruthenium nickel alloy aerogel.
[0056] 2. Put the ruthenium-nickel alloy aerogel into a quartz boat and send it into the reaction chamber. Under Ar protection, heat the reaction chamber to 400°C at a heating rate of 5°C / min and keep it warm for 50 minutes.
[0057] 3. Continue to introduce a mixed gas of Ar, H2 and C2H4 into the reaction chamber for 50 min to obtain a black solid, and then obtain a composite material of ruthenium nickel alloy aerogel in situ grown carbon nanotubes; wherein the flow ratio of Ar, H2 and C2H4 in the mixed gas is 1:2:1. The SEM image of the obtained aerogel in situ grown carbon nanotubes is shown in Fig. 9 shown. Example
[0058] 1. First, take 10 ml of the prepared 188 mM NiCl2 aqueous solution and add it to 100 ml of deionized water. After stirring and dispersing it evenly with a magnetic stirrer, add 3 ml of 1 M NaBH4 solution. The solution quickly turns black. After removing the magnetic stirrer and standing for 2-8 hours, the black gel will settle at the bottom of the container or float on the solution. The obtained gel is purified 6-8 times with a large amount of deionized water, and the total purification time is 2-3 days. Then, the gel is solvent exchanged with tert-butanol at 303 K for 3-4 times, and the exchange time is 2 days. After that, the gel is quickly frozen with liquid nitrogen and kept at 77 K for about 10-15 min. Finally, the frozen sample is freeze-dried at about 1 Pa and -80 ° C for 12-24 h to obtain Ni aerogel.
[0059] 2. Place the Ni metal aerogel in a quartz boat and place it in the reaction chamber. Heat the reaction chamber to 660°C at a heating rate of 5°C / min under N2 protection and keep it warm for 45 min.
[0060] 3. A mixed gas of N2, H2 and C3H6 was continuously introduced into the reaction chamber for 0.25 h to obtain a black solid; the flow ratio of N2, H2 and C3H6 in the mixed gas was 3:4:1. SEM image of the obtained aerogel with in-situ growth of carbon nanotubes. Both the aerogel and carbon nanotubes mentioned above exist and are perfectly combined. Example
[0061] 1. First, take 10 ml of the prepared 325 mM FeCl3 and NiCl2 aqueous solutions and add them to 100 ml of deionized water in turn. After stirring and dispersing them evenly with a magnetic stirrer, add 40 ml of 0.5 M NaBH4 solution and 10 ml of 10 M NH4F solution in turn. The solution quickly turns black. After removing the magnetic stirrer and standing for 2-8 hours, the black gel will be deposited at the bottom of the container or float on the solution. The obtained gel is purified 6-8 times with a large amount of deionized water, and the total purification time is 2-3 days. Then, the gel is solvent exchanged with tert-butanol for 3-4 times at 303 K, and the exchange time is 2 days. After that, the gel is quickly frozen with liquid nitrogen and kept at 77 K for about 10-15 min. Finally, the frozen sample is freeze-dried at about 1 Pa and -80 ° C for 12-24 h to obtain nickel-iron alloy aerogel.
[0062] 2. Place the nickel-iron alloy aerogel in a quartz boat and send it into the reaction chamber. Heat the reaction chamber to 400°C at a heating rate of 5°C / min under Ar protection and keep it warm for 50 min.
[0063] 3. Continue to introduce a mixed gas of Ar, H2 and C2H4 into the reaction chamber for 50 min to obtain a black solid, and then obtain a composite material of in-situ growth of carbon nanotubes on nickel-iron alloy aerogel; wherein the flow ratio of Ar, H2 and C2H4 in the mixed gas is 1:2:1. The SEM image of the obtained aerogel in-situ growth of carbon nanotubes is shown.
[0064] Through the above embodiments, it can be concluded that:
[0065] First, the present invention provides a method for preparing carbon nanotubes by in-situ growth of metal aerogels, which can effectively and stably obtain finished products.
[0066] Second, through the instructions attached Figure 6 It can be proved that both aerogel and carbon nanotubes exist and are perfectly combined together.
[0067] third, Figure 8 , 9 This reflects the inventor's regulation of the growth method through experiments, which echoes the performance regulation mentioned above.
[0068] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that a technician familiar with the technical field can think of within the technical scope disclosed in the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for preparing metal aerogel in-situ grown carbon nanotubes, characterized in that: The steps include: Step 1: introducing a metal solution, a solvent, a ligand solution, a reducing agent, and an initiator into a reaction vessel, and then changing the external conditions to make it self-assemble to form a metal hydrogel, and then washing it multiple times and exchanging it with an alcohol solution for freeze drying to obtain a metal aerogel; wherein the freeze drying temperature is 0-77 K; Step 2: Place the obtained metal aerogel into a reaction chamber, and heat the reaction chamber to 300°C-1500°C under inert gas protection, and keep the temperature for 30 min-60 min; Step 3, continuously introducing reducing gas, inert gas and gaseous carbon-containing organic matter into the reaction chamber, and continuously reacting to obtain a composite material of metal aerogel in-situ grown carbon nanotubes; The ratio of reducing gas, inert gas and gaseous carbon-containing organic matter is 0.1-10:1:0.01-50; The metal solution in step 1 is a mixture of one or more metal solutions of iron, cobalt, nickel, copper, ruthenium and rhodium in any proportion; The composite material in step three uses metal aerogel as a framework and catalyst to control the growth of carbon nanotubes in its 3D structure to form a three-dimensional macroscopic, self-supporting network structure of metal aerogel-carbon nanotubes; wherein, step one adjusts the physical properties of the metal aerogel by changing the pressure; the pressure range in step one is 1Pa-100 MPa; wherein, the physical properties of the metal aerogel in step one include shape, density, pores and spacing.
2. The preparation method according to claim 1, characterized in that in, Step 2: The heating rate of the reaction chamber is 3°C / min-40°C / min.
3. The preparation method according to claim 1, characterized in that: in, The inert gas in step 2 is one or more of nitrogen, argon or helium.
4. The preparation method according to claim 1, characterized in that: The reaction chamber in step 2 is a vertical tube furnace or a horizontal tube furnace.
5. The preparation method according to claim 1, characterized in that: The inert gas in step three is one or more of nitrogen, argon or helium; the gaseous carbon-containing organic matter is carbon-containing organic gas or vaporized organic liquid, and the vaporization temperature of the organic liquid is 100°C-300°C.
6. The preparation method according to claim 5, characterized in that: In step three, the carbon-containing organic gas is one or a mixture of methane, natural gas, ethane, ethylene, acetylene, propane, and propylene; the vaporized organic liquid is one or a mixture of anhydrous methanol, anhydrous ethanol, benzene, toluene, and xylene.