Air layer suede fabric and preparation process thereof
By using quaternary ammonium salt catalysts and chitosan quaternary ammonium salts in the alkali reduction and dyeing process of air-layer suede fabrics, the problem of large color difference after dyeing of sea-island fibers and low-elastic fibers has been solved and achieved More uniform dyeing and improved rub resistance.
Patent Information
- Application Number
- CN202310008036.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-01-04
AI Technical Summary
During the dyeing process of air-layer suede fabrics, due to the structural differences between island fibers and low-elastic fibers, the color difference between the upper surface layer and the lower surface layer is large, affecting the consistency and quality of its color.
Quaternary ammonium salt catalysts and low-concentration sodium hydroxide solutions are used to reduce surface tension during the alkali reduction process, increase the hydrophilicity of the fiber, and allow the dye to penetrate into the low-elastic fiber more evenly; at the same time, chitosan quaternary ammonium salt and carboxylic acid are used Methylcellulose is used to control the adsorption position of dye and reduce color difference.
It effectively reduces the color difference between the upper and lower surface layers of air-layer suede fabrics, improves color consistency and rubbing fastness after dyeing, and reduces fiber damage and decrease in breaking strength.
Smart Images

Figure GDA0005031512010000061 
Figure GDA0005031512010000071 
Figure GDA0005031512010000072
Abstract
Description
Technical Field
[0001] The invention relates to the field of cloth dyeing and finishing, in particular to an air layer suede fabric and a preparation process thereof. Background Art
[0002] Air layer suede fabric is now more and more widely used in people's lives. It has the characteristics of being thick, soft, fine velvety, and having good elasticity. It is an ideal fabric for high-end women's trousers, fashionable women's jackets and car interiors.
[0003] Air layer suede fabrics are now available on the market. Generally, they are made of sea island fiber and low-elastic fiber as raw materials, and are produced by double-sided knitting machines to make grey cloth. The prepared grey cloth is produced through processes such as pre-shrinking, alkali reduction, fiber opening, pre-shaping, brushing, sanding, and dyeing to produce air suede fabrics.
[0004] However, the upper surface of the air layer suede fabric is sea island fiber, which has a fluffy structure. When the sea island fiber is dyed, the dye can easily penetrate into the interior of the sea island fiber, which reduces the apparent depth of the upper surface of the air layer suede fabric; while the lower surface of the air layer suede fabric is low-elastic fiber, which does not have the fluffy structure of the sea island fiber, and the dye can easily adhere to the surface of the low-elastic fiber molecules, which increases the apparent depth of the lower surface of the air layer suede fabric, resulting in a large color difference between the upper and lower surfaces of the air layer suede fabric after dyeing. Summary of the invention
[0005] In order to improve the problem of large color difference between the upper surface layer and the lower surface layer of the air layer suede fabric after dyeing, the present application provides an air layer suede fabric and a preparation process thereof.
[0006] In the first aspect, a processing technology for air layer suede fabric adopts the following technical solution:
[0007] A processing process for air layer suede fabric comprises the following steps:
[0008] S1 grey cloth → S2 pre-shrinkage → S3 flattening → S4 alkali reduction → S5 sanding → S6 dyeing → S7 dehydration and opening → S8 shaping → S9 brushing → S10 inspection and curling;
[0009] The fabric obtained from the grey cloth in step S1 comprises an upper surface layer and a lower surface layer, wherein the upper surface layer is a sea-island fiber layer, and the low-elastic polyester fiber and the spandex fiber are spun and woven to obtain the lower surface layer;
[0010] The alkali reduction step S4 is to treat the grey cloth with an alkali reduction mixed solution, wherein the alkali reduction mixed solution includes a quaternary ammonium salt catalyst, sodium hydroxide and water, the concentration of the sodium hydroxide is 1-7 g / L, the alkali reduction time is 40-90 min, and the alkali reduction temperature is 100-110° C.;
[0011] The dyeing raw materials used in the dyeing step S6 include: 1.5-2.5 g / L of disperse dye, 0.3-0.8 g / L of dispersant, 1.0-2.0 g / L of leveling agent, 0.8-1.2 g / L of acetic acid, and 0.1-0.3 g / L of chitosan quaternary ammonium salt.
[0012] By adopting the above technical scheme, in the alkali reduction step of the treatment process of the air layer suede fabric, a quaternary ammonium salt catalyst is used in combination with a low concentration of sodium hydroxide solution. During the alkali reduction process of the sea island fiber and the low-elastic polyester, under the action of the quaternary ammonium salt catalyst, the surface tension of the alkali reduction mixture is reduced, the hydrophilicity of the grey cloth fiber is increased, and the alkali reduction mixture is easier to penetrate into the interior of the grey cloth fiber molecules, so that the alkali reduction of the ordinary low-elastic polyester fiber is more uniform and the structure of the dyed area of the fiber molecules is more fluffy.
[0013] When the blank is dyed after the above-mentioned alkali reduction, the molecular structure of the ordinary low-elastic polyester fiber becomes more fluffy, allowing more dyes to enter the interior of the ordinary low-elastic polyester molecules instead of gathering on the fiber molecules or the surface of the blank, making the color of the upper and lower surfaces of the air layer suede fabric closer, thereby reducing the color difference between the upper and lower surfaces of the air layer suede fabric.
[0014] In the S6 dyeing step, the blank to be colored is treated with chitosan quaternary ammonium salt. The chitosan quaternary ammonium salt and the alkali-reduced carboxyl groups of the blank are attracted and combined with each other, so that the ends of the blank fiber molecules are connected to multiple easily dyed hydroxyl groups, so that when the island fiber is dyed, more dyes are adsorbed on the surface of the island fiber instead of entering the interior of the island fiber, thereby reducing the color difference between the upper and lower surfaces of the air layer suede fabric after dyeing.
[0015] Preferably, the concentration of the quaternary ammonium salt catalyst is 1-1.5 g / L, the concentration of sodium hydroxide during the alkali reduction treatment is 2-5 g / L, and the alkali reduction time is 50-75 min.
[0016] By adopting the above technical scheme, when the concentration of the quaternary ammonium salt catalyst is 1-1.5g / L, the concentration of sodium hydroxide during alkali reduction treatment is 2-5g / L, and the alkali reduction time is 50-70min, the quaternary ammonium salt catalyst and the low-concentration alkali reduction mixed solution cooperate with each other, and the alkali reduction mixed solution is more likely to penetrate into the interior of the ordinary low-elastic polyester fiber, thereby increasing the hydrolysis of the fiber molecules inside the ordinary low-elastic polyester fiber, so that the structure between the fiber molecules of the ordinary low-elastic polyester fiber after alkali reduction is relatively more fluffy, so that the dye does not accumulate on the fiber molecules and the fabric surface after dyeing, so that the colors of the upper and lower surfaces of the air layer suede fabric are closer.
[0017] When the concentration of sodium hydroxide is too high, there is excessive alkali reduction and the alkali reduction on the surface of ordinary low-elastic polyester fibers is large, the alkali reduction inside ordinary low-elastic polyester fibers is small, the structure between ordinary low-elastic polyester fiber molecules is not fluffy enough, and the dye is concentrated on the surface of ordinary low-elastic polyester fiber molecules, resulting in an increase in the color difference between the upper and lower surfaces of the air layer suede fabric.
[0018] Optionally, after the alkali reduction in S4, the grey fabric after alkali reduction is left to stand for 3-7 hours and then subjected to sanding treatment.
[0019] Through the above technical scheme, after the alkali reduction in S4, the grey cloth after alkali reduction is allowed to stand, so that the residual sodium hydroxide, moisture and ester bonds of the fibers in the grey cloth are further reduced by alkali, so that the alkali reduction of ordinary low-elastic polyester fibers is more uniform, and the structure of the dyed area of the fiber molecules is more fluffy, thereby reducing the color difference between the upper and lower surfaces of the air layer suede fabric. On the other hand, the grey cloth after alkali reduction is allowed to stand so that the sanding effect of the grey cloth in the subsequent sanding step is better.
[0020] Optionally, the alkali-reduced mixed solution further includes an aliphatic polyol, and the concentration of the aliphatic polyol is 3-5 g / L.
[0021] Through the above technical scheme, aliphatic polyols are good wetting agents and penetrants, and have strong permeability in grey cloth fibers. When the grey cloth is alkali-reduced, more alkali-reduced mixed liquid and quaternary ammonium salt catalyst penetrate into the ordinary low-elastic polyester fiber, so that the structure between fiber molecules of the ordinary low-elastic polyester fiber after alkali reduction is relatively more fluffy, so that the dye does not gather on the surface of the fiber molecules, and the colors of the upper and lower surfaces of the air layer suede fabric after dyeing are closer.
[0022] Preferably, the dyeing raw material in the dyeing step S6 also includes carboxymethyl cellulose.
[0023] By adopting the above technical scheme, the blank to be colored is treated with carboxymethyl cellulose and chitosan quaternary ammonium salt, the carboxyl group on the carboxymethyl cellulose forms a hydrogen bond or reacts with the hydroxyl group formed after alkali reduction, the chitosan quaternary ammonium salt and the carboxyl group formed after alkali reduction have opposite charges and attract each other, so that a plurality of easily dyeable hydroxyl groups are introduced into the sea island fiber molecules, and the carboxymethyl cellulose and the polysaccharide quaternary ammonium salt act synergistically to allow more dyes to be adsorbed on the surface of the sea island fiber, thereby reducing the color difference between the upper and lower surfaces of the air layer suede fabric after dyeing.
[0024] Preferably, in the dyeing step S6, the carboxymethyl cellulose is added in a priority order over the chitosan quaternary ammonium salt, and the chitosan quaternary ammonium salt is added in a priority order over the dispersant.
[0025] By adopting the above technical scheme, the addition order of carboxymethyl cellulose takes precedence over chitosan quaternary ammonium salt, and the addition order of chitosan quaternary ammonium salt takes precedence over dispersant, thereby reducing the mutual interference of carboxymethyl cellulose and chitosan quaternary ammonium salt added at the same time, so that carboxymethyl cellulose and chitosan quaternary ammonium salt can be better combined with the hydrolyzed groups on the grey cloth after alkali reduction.
[0026] Preferably, in the dyeing step S6, the molar ratio of chitosan quaternary ammonium salt to carboxymethyl cellulose in the dyeing raw material is (0.6-1):1.
[0027] By adopting the above technical scheme, when the molar ratio of chitosan quaternary ammonium salt to carboxymethyl cellulose is (0.6-1):1, the synergy between chitosan quaternary ammonium salt and carboxymethyl cellulose is the greatest, and after interacting with the grey cloth after alkali reduction, more hydroxyl groups that can combine with the dye are connected to the grey cloth after alkali reduction, and more dyes are adsorbed on the surface of the sea island fiber, thereby improving the large color difference between the upper and lower surfaces of the air layer suede fabric after dyeing; if the molar ratio of chitosan quaternary ammonium salt to carboxymethyl cellulose is too large or too small, more hydroxyl groups that can combine with the dye are connected to the grey cloth after alkali reduction.
[0028] Preferably, in the dyeing step S6, the molar ratio of chitosan quaternary ammonium salt to carboxymethyl cellulose in the dyeing raw material is (0.6-1):1.
[0029] By adopting the above technical scheme, the dye is wrapped and dispersed by a mixture of amphoteric surfactants and non-ionic surfactants, and has a good affinity with the carboxylic acid after hydrolysis of the grey cloth, the quaternary ammonium salt of chitosan and carboxymethyl cellulose, and the alkyl groups on the fiber molecules. The amphoteric surfactants and non-ionic surfactants work better together, so that more dyes are adsorbed on the surface of the sea island fiber, thereby improving the large color difference between the upper and lower surfaces of the air layer suede fabric after dyeing.
[0030] In a second aspect, the present application provides an air layer suede fabric, which is composed of the following raw materials: 35-45 parts of sea island fibers;
[0031] 47-57 parts of low-elastic polyester fiber;
[0032] 6-10 parts of spandex fiber;
[0033] The grey cloth comprises an upper surface layer and a lower surface layer, wherein the upper surface layer is a sea-island fiber layer, and the low-elastic polyester fiber and spandex fiber are woven to obtain the lower surface layer.
[0034] By adopting the above technical scheme, the sea island fiber gives the air layer suede fabric a soft feel, rich hair effect, good air permeability and wrinkle resistance; low-elastic polyester fiber and spandex fiber are used as the raw materials for the lower surface layer, and the spandex fiber and the low-elastic polyester fiber are co-woven, which gives the lower surface layer of the air layer suede fabric good elasticity, so that the entire air layer suede fabric has good elasticity; low-elastic polyester fiber and sea island fiber are both polyester fibers, and compared with other fiber yarns, the color difference between the low-elastic polyester fiber and the sea island fiber after coloring is smaller, and during color modification, the two are modified simultaneously, thereby improving the large color difference between the upper and lower surfaces of the air layer suede fabric after dyeing.
[0035] In summary, this application has the following beneficial effects:
[0036] 1. In the alkali reduction process of the treatment process of the air layer suede fabric, quaternary ammonium salt catalysts are used, combined with low-concentration sodium hydroxide solution and added aliphatic polyols, so that more alkali reduction mixture and quaternary ammonium salt catalyst penetrate into the ordinary low-elastic polyester fiber, making the alkali reduction of ordinary low-elastic polyester more uniform, and the structure of the fiber molecule dyeing area is more fluffy, so that the dye can more easily enter between the ordinary low-elastic polyester fiber molecules, thereby reducing the color rendering of the lower surface of the air layer suede fabric, and reducing the color difference between the upper and lower surfaces of the air layer suede fabric after dyeing. At the same time, the low-concentration sodium hydroxide solution makes the alkali reduction of the fiber molecules more uniform and reduces the damage to the fiber, reducing the decrease in the breaking strength of the air layer suede fabric.
[0037] 2. In the S6 dyeing step, chitosan quaternary ammonium salt and carboxymethyl cellulose are used to treat the blank to be colored, so that multiple hydroxyl groups are connected to the alkali-reduced groups of the fiber molecules of the blank. During dyeing, more dyes are adsorbed on the surface of the fiber molecules instead of entering the interior of the fluffy sea-island fibers, thereby reducing the color difference between the upper and lower surfaces of the air layer suede fabric after dyeing.
[0038] 3. During S6 dyeing, the dye is wrapped and dispersed by a mixture of amphoteric surfactants and nonionic surfactants, so that the dye can be better combined with the grey cloth, so that more dye is adsorbed on the surface of the sea island fiber, thereby reducing the color difference between the upper and lower surfaces of the air layer suede fabric after dyeing. DETAILED DESCRIPTION
[0039] Raw materials: sea island fiber (215d / 84f), low-elastic polyester fiber (88d / 36f), spandex fiber (76d / 36f), leveling agent (model: RG-HD100), hydroxymethyl cellulose (CAS: 9000-11-7), chitosan quaternary ammonium salt (CAS: 70694-72-3), lauryl hydroxysulfobetaine (CAS: 13197-76-7), lecithin (CAS: 8002-43-5), alkyl Phenol polyoxyethylene ether (CAS: 14409-72-4), Tween 60 (CAS: 9005-67-8), Disperse Navy 2G-SF (Dye Index: DB270), Disperse Red F3BS (CAS: 99031-78-6), Dodecylmethylbenzylammonium bromide (CAS: 7281-04-1), Tetrabutylammonium chloride (CAS: 37451-68-6), and Hydrosulfite (CAS: 7775-14-6).
[0040] Example
[0041] Example 1
[0042] A processing process for air layer suede fabric comprises the following steps:
[0043] S1 grey cloth → S2 pre-shrinkage → S3 flattening → S4 alkali reduction → S5 sanding → S6 dyeing → S7 dehydration and opening → S8 shaping → S9 brushing → S10 inspection and curling;
[0044] Among them, S1 grey cloth: with sea island fiber, low-elastic polyester fiber and spandex fiber as raw materials, the grey cloth is woven on a 72-needle double-sided knitting machine. The upper surface layer of the grey cloth is the sea island fiber layer, and the lower surface layer of the grey cloth is the low-elastic polyester fiber. 10kg of grey cloth is obtained, in which the weight ratio of the sea island fiber, low-elastic polyester fiber and spandex fiber is 35:47:10, and the gram weight of the grey cloth is 280g / m2.
[0045] S2 preshrinking: The S2 flattened grey cloth is sent to the flat-width preshrinking machine for completion. In the flat-width preshrinking machine, three water tanks with temperatures of 60°C, 70°C and 90°C are arranged in sequence along the forward direction of the cloth. The cloth feeding speed is 45m / min.
[0046] S3 leveling: The grey cloth is transported to the leveling machine for leveling at a temperature of 180°C and a leveling time of 20 minutes.
[0047] S4 alkali reduction: send the grey cloth after S3 pre-shrinking machine into the 200L alkali reduction mixed solution of the padding machine. The alkali reduction mixed solution is a mixture of quaternary ammonium salt catalyst, ethylene glycol, sodium hydroxide and water, wherein the quaternary ammonium salt catalyst is dodecylmethylbenzylammonium bromide, the concentration of dodecylmethylbenzylammonium bromide is 1g / L, the concentration of ethylene glycol is 3g / L, the concentration of sodium hydroxide is 1g / L, the temperature is 100℃, the bath ratio is 1:20, the treatment time is 90min, then the grey cloth is taken out of the bathtub and drained, after draining, the grey cloth is left to stand at 25℃ for 3h, and then washed with water at 60℃ for 10min.
[0048] S5 sanding: The grey cloth after S4 alkali reduction and standing is sent into the sanding machine. Four guide rollers are arranged in sequence along the forward direction of the cloth on the sanding machine. The outer walls of the four guide rollers are covered with a layer of sandpaper. The sandpaper of the four guide rollers is 500 mesh, 400 mesh, 400 mesh and 600 mesh respectively. The rotation speed of the guide roller is 1200 rpm.
[0049] S6 dyeing: the brushed grey cloth is immersed in 100L dyeing solution with a bath ratio of 1:10, and dyed with a high temperature and high pressure overflow dyeing machine. The dyeing solution is a mixture of the following raw materials, water and ethanol, wherein the volume ratio of ethanol to water is 1:5; the dyeing solution contains the following raw materials and their concentrations: 1.5g / L disperse dye, 1.0g / L leveling agent, 0.8g / L acetic acid, 0.8g / L dispersant, 0.1g / L chitosan quaternary ammonium salt and 0.125g / L carboxymethyl cellulose, and the molar ratio of chitosan quaternary ammonium salt to carboxymethyl cellulose is 0.8:1.
[0050] The dispersant includes lauryl hydroxysulfonyl betaine and alkylphenol polyoxyethylene ether, and the molar ratio of lauryl hydroxysulfonyl betaine to alkylphenol polyoxyethylene ether is 0.4:1.
[0051] The dyeing process is divided into three stages: ① pre-dyeing stage, the temperature is 48°C; ② dyeing stage: after the pre-dyeing stage, the temperature is raised to 130°C at a rate of 1.5°C / min and maintained for 45 minutes; ③ reduction cleaning: after the dyeing stage, the temperature is lowered to 70°C at a rate of 2°C / min and reduction cleaning is performed for 20 minutes.
[0052] The order of adding materials in the pre-dyeing stage is carboxymethyl cellulose, chitosan quaternary ammonium salt, leveling agent, acetic acid, dodecyl ethoxy sulfobetaine and alkylphenol polyoxyethylene ether, and disperse dye.
[0053] In the reduction cleaning stage, the cleaning agents used were sodium hydroxide 1.2% (owf); sodium hydrosulfite 3g / L.
[0054] S7 Dehydration and Width Opening: The grey cloth after reduction cleaning is transported to the dehydrator for dehydration, and then transported to the width opening machine for width opening.
[0055] S8 setting: put the grey cloth after S7 dehydration and opening into the heat setting machine, then adjust the temperature of the heat setting machine to 170℃, keep warm for 45s, cool after heat setting, the cooling temperature is 25℃, and the cooling time is 40min.
[0056] S9 brushing: the grey cloth obtained in step S8 is brushed by a brushing machine, and the speed of the brushing process is 3-6 m / min.
[0057] S10 inspection and rolling.
[0058] Example 2-3
[0059] The difference from Example 1 is that the weight of the raw materials of the grey cloth is different; in the S4 alkali reduction process, the concentrations of the quaternary ammonium salt catalyst, ethylene glycol and sodium hydroxide are different, and the alkali reduction time and alkali reduction temperature are different; in the S6 dyeing process, the concentrations of the disperse dye, dispersant and chitosan quaternary ammonium salt are set differently. The details are shown in Table 1:
[0060] Table 1 Parameter list of Examples 1-3 S4 reduction and S6 dyeing
[0061]
[0062]
[0063] The difference from Example 2 is that the concentration of sodium hydroxide in the S4 alkali reduction step is set differently, as shown in Table 2:
[0064] Table 2 Parameter list of sodium hydroxide concentration of Examples 4-7 and Example 2
[0065]
[0066] Embodiment 8-11
[0067] The difference from Example 2 is that the alkali reduction time in the S4 alkali reduction step is set differently, as shown in Table 3:
[0068] Table 3 Parameter list of alkali reduction time of Examples 8-11 and Example 2
[0069]
[0070] Example 12
[0071] The difference from Example 2 is that an equal amount of propylene glycol is used to replace ethylene glycol in the alkali reduction mixed solution in the S4 alkali reduction step.
[0072] Embodiment 13
[0073] The difference from Example 2 is that ethylene glycol is not used in the alkali reduction mixed liquid in the S4 alkali reduction step.
[0074] Embodiment 14
[0075] The difference from Example 2 is that the dodecylmethylbenzylammonium bromide is replaced by an equal amount of tetrabutylammonium chloride in the alkali reduction mixed solution in the alkali reduction step S4.
[0076] Examples 15-18
[0077] The difference from Example 2 is that in the S6 dyeing step, when the concentration of the chitosan quaternary ammonium salt is 0.2 g / L, the molar ratio of the chitosan quaternary ammonium salt and the carboxymethyl cellulose is set differently, as shown in Table 4:
[0078] Table 4 Parameter list of the molar ratio of chitosan quaternary ammonium salt and carboxymethyl cellulose in Examples 15-18 and Example 2
[0079]
[0080] Embodiment 19
[0081] The difference from Example 2 is that in the S6 dyeing step, an equal amount of chitosan quaternary ammonium salt is replaced by carboxymethyl cellulose.
[0082] Embodiment 20
[0083] The difference from Example 2 is that in the S6 dyeing step, an equal amount of carboxymethyl cellulose is replaced by chitosan quaternary ammonium salt.
[0084] Embodiment 21
[0085] The difference from Example 2 is that in the S6 dyeing step, the order of adding materials in the pre-dyeing stage is carboxymethyl cellulose & chitosan quaternary ammonium salt & dispersant, acetic acid, and disperse dye.
[0086] Examples 22-25
[0087] The difference from Example 2 is that in the S6 dyeing step, when the dispersant includes lauryl hydroxysulfonyl betaine and alkylphenol polyoxyethylene ether and the concentration of the dispersant is 0.5 g / L, the molar ratio of lauryl hydroxysulfonyl betaine to alkylphenol polyoxyethylene ether is set differently, as shown in Table 5:
[0088] Table 5 Parameter list of the molar ratio of lauryl hydroxysulfobetaine to alkylphenol polyoxyethylene ether in Examples 22-25 and Example 2
[0089]
[0090] Embodiment 26
[0091] The difference from Example 2 is that in the S6 dyeing step, the dispersant is lauryl hydroxysulfonyl betaine, and the concentration of lauryl hydroxysulfonyl betaine is 0.5 g / L.
[0092] Embodiment 27
[0093] The difference from Example 2 is that in the S6 dyeing step, the dispersant is alkylphenol polyoxyethylene ether, and the concentration of alkylphenol polyoxyethylene ether is 0.5 g / L.
[0094] Embodiment 28
[0095] The difference from Example 2 is that in the S6 dyeing step, Tween 60 is used to replace the alkylphenol polyoxyethylene ether in an equal amount.
[0096] Embodiment 29
[0097] The difference from Example 2 is that in the S6 dyeing step, lecithin is replaced by an equal amount of dodecylethoxysulfobetaine.
[0098] Embodiment 30
[0099] The difference from Example 2 is that the grey cloth is not left to stand after S4 alkali reduction and before sanding, but sanding is performed directly after the water is wrung out.
[0100] Comparative Example
[0101] Comparative Example 1
[0102] The difference from Example 2 is that no quaternary ammonium salt catalyst is used in the alkali reduction mixed solution.
[0103] Comparative Example 2
[0104] The difference from Example 2 is that the dyeing raw material used in step S6 for dyeing does not use chitosan quaternary ammonium salt.
[0105] Comparative Example 3
[0106] The difference from Example 2 is that the concentration of sodium hydroxide in the alkali reduction mixed solution is 18 g / L, and no quaternary ammonium salt catalyst is used.
[0107] Comparative Example 4
[0108] The difference from Example 2 is that the concentration of sodium hydroxide in the alkali reduction mixed solution is 18 g / L, the alkali reduction time is 40 min, and a quaternary ammonium salt catalyst is used.
[0109] Comparative Example 5
[0110] The difference from Example 2 is that no quaternary ammonium salt catalyst and ethylene glycol are used in the alkali reduction mixed solution.
[0111] Performance testing
[0112] 1. Color difference grade determination: Referring to GB / T250-2008 "Gray Scale for Color Fastness Tests and Evaluation of Color Change in Textiles", the color difference of the upper and lower surfaces of the dyed fabrics of the above-mentioned embodiment and comparative example was tested to obtain the color difference grade of the upper and lower surfaces.
[0113] 2. Color fastness to rubbing: The color fastness to rubbing was tested by a rubbing fastness tester in accordance with GB / T3920-2008 “Textiles - Color fastness - Rubbing color fastness” on the dyed upper surface of the fabrics in the above-mentioned embodiments and comparative examples, and then rated using GB / T250-2008 “Grey Scale for Assessing Discoloration”.
[0114] According to the processing technology of the air layer suede fabric of the above-mentioned Examples 1-29 and Comparative Examples 1-7, disperse dyes are dispersed navy blue 2G-SF and disperse red F3BS. After the grey cloth is dyed, the dyeing performance is tested according to the above-mentioned color difference grade and rubbing color fastness standards, and the results are recorded. The test results are shown in Table 6.
[0115] Table 6 Test results of color difference grade and color fastness to friction of air layer suede fabrics of Examples 1-29 and Comparative Examples 1-7
[0116]
[0117]
[0118] 3. Breaking strength: refer to GB / T3923.1-2013 “Tensile properties of textile fabrics Part 1: Determination of breaking strength and elongation at break (strip method)”, measure on an electronic fabric strength meter, measure three times in parallel and take the average value.
[0119] The fabric was tested for performance according to the above standards and the results were recorded. The test results are shown in Table 7.
[0120] Table 7 Test results of breaking strength of air layer suede fabrics of embodiments and comparative examples related to breaking strength
[0121] distinguish Warp breaking strength / N distinguish Warp breaking strength / N Example 2 575 Embodiment 11 568 Example 4 582 Embodiment 13 578 Example 5 579 Comparative Example 30 575 Example 6 572 Comparative Example 1 580 Example 7 567 Comparative Example 3 549 Example 8 585 Comparative Example 4 535 Example 9 580 Comparative Example 5 582 Example 10 575 - -
[0122] Combining Examples 1-3 and Comparative Example 1 and Table 6, it can be seen that:
[0123] In the dyeing of air layer suede fabric, quaternary ammonium salt catalyst is added in combination with low concentration sodium hydroxide solution in the S4 alkali reduction process to make the alkali reduction of ordinary low-elastic polyester fiber more uniform, the structure of the dyeing area of the fiber molecules more fluffy, and the dye can more easily enter between the low-elastic polyester fiber molecules, so that the color difference between the upper and lower surfaces of the air layer suede fabric is reduced, and the friction color fastness of the upper surface of the air layer suede fabric is increased.
[0124] Combining Examples 4-11 and Comparative Example 1 with Table 6, it can be seen that:
[0125] In the S4 alkali reduction process, under the action of quaternary ammonium salt catalysts, the appropriate alkali reduction mixed liquid concentration and alkali reduction mixed liquid time are used to reduce the color difference between the upper and lower surfaces of the air layer suede fabric. This may be because under the action of quaternary ammonium salt catalysts, the grey cloth fiber molecules are hydrolyzed at a lower concentration of sodium hydroxide, the alkali reduction of the fibers is more uniform, and the dye can more easily enter the low-elastic polyester fiber, which reduces the color difference between the upper and lower surfaces of the air layer suede fabric.
[0126] When the concentration of the alkali solution in the alkali reduction mixture is too high, the alkali reduction on the surface of the low-elastic polyester fiber will increase, the dyeing degree will increase, the color fastness to rubbing will increase, and the color difference between the upper and lower surfaces of the air layer suede fabric will increase; when the concentration of the alkali solution in the alkali reduction mixture is too low, or the alkali reduction time is too short, there is insufficient alkali reduction of the low-elastic polyester fiber, the dye is easily accumulated on the surface of the low-elastic polyester fiber, the color difference between the upper and lower surfaces of the air layer suede fabric will increase, and the color fastness to rubbing will decrease.
[0127] Combining Example 13, Example 2, Comparative Example 1 and Comparative Example 5, and Table 6, it can be seen that the addition of ethylene glycol and quaternary ammonium salt catalysts during the S4 alkali reduction process reduces the color difference between the upper and lower surfaces of the air layer suede fabric. The reduction in color fastness of Comparative Examples 1 and 5 may be due to insufficient alkali reduction of the fiber of the air layer suede fabric.
[0128] In combination with Examples 15-20, Example and Comparative Example 2, and in combination with Table 6, it can be seen that the appropriate ratio of chitosan quaternary ammonium salt and carboxymethyl cellulose can reduce the color difference between the upper and lower surfaces of the air layer suede fabric, and increase the color fastness to friction. This may be because the chitosan quaternary ammonium salt and carboxymethyl cellulose are combined with the hydrolyzed groups of the fiber molecules on the grey cloth, and synergistically increase the hydroxyl groups of the easily dyeable groups on the surface of the sea-island silk fibers and enhance the binding force between the dyeing groups and the grey cloth; when the ratio of chitosan quaternary ammonium salt and carboxymethyl cellulose is too large or too small, the hydroxyl groups of the easily dyeable groups connected to the surface of the sea-island silk fibers are reduced, which increases the color difference between the upper and lower surfaces of the air layer suede fabric and reduces the color fastness to friction.
[0129] Combining Examples 22-27 and Example 2, and Table 6, it can be seen that when the amphoteric surfactant and the nonionic surfactant are in a suitable ratio, the color difference between the upper and lower surfaces of the air layer suede fabric is reduced, which may be because the amphoteric surfactant and the nonionic surfactant cooperate with the carboxymethyl cellulose and the chitosan quaternary ammonium salt, so that the hydroxyl groups on the surface of the sea island fiber that are easy to dye increase, and then the surface of the sea island fiber is connected with more dyes, so that the color difference between the upper and lower surfaces of the air layer suede fabric is reduced. When the hydroxyl groups on the surface of the sea island fiber that are easy to dye increase, the friction color fastness of the sea island fiber increases.
[0130] Combining Examples 4-11 and Example 2, and combining Tables 6-7, it can be seen that:
[0131] As the degree of alkali reduction of the air layer suede fabric increases, that is, the concentration of the alkali solution in the alkali reduction step increases or the alkali reduction time is prolonged, the warp breaking strength of the air layer suede fabric decreases; while a lower alkali solution concentration and a suitable alkali reduction time can make the alkali reduction of the ordinary low-elastic polyester fiber of the grey cloth more uniform, and reduce the color difference between the upper and lower surfaces of the air layer suede fabric; on the other hand, a lower alkali solution concentration and a suitable alkali reduction time reduce fiber damage, so that the breaking strength of the air layer suede fabric does not decrease significantly.
[0132] In combination with Example 13, Example 2, Comparative Example 1 and Comparative Examples 4-5, and in combination with Table 7, it can be seen that when ethylene glycol and quaternary ammonium salt catalysts are used in combination, the warp breaking strength of the air layer suede fabric does not decrease significantly while ensuring the degree of alkali reduction. In other words, the combined use of ethylene glycol and quaternary ammonium salt catalysts has a certain protective effect on the air layer suede fabric, reducing the reduction in the warp breaking strength of the blank during the alkali reduction process. This may be because the combination of ethylene glycol and quaternary ammonium salt catalysts in low concentration alkali solution makes the alkali reduction of the grey cloth more uniform, causing less damage to the fiber.
[0133] Combining Example 2 and Example 30, and combining Tables 6-7, it can be seen that
[0134] The alkali-reduced grey fabric was left standing to reduce the color difference between the upper and lower surfaces of the air layer suede fabric, and the color fastness of the upper surface was increased. This may be because the alkali reduction of the fiber molecules of the grey fabric was more uniform after the alkali-reduced grey fabric was left standing, while the breaking strength of the air layer suede fabric was almost unchanged.
[0135] Combining Example 2, Comparative Example 1 and Comparative Example 5, and combining Tables 6-7, it can be seen that:
[0136] In Comparative Examples 1 and 5, since no quaternary ammonium salt catalyst and / or ethylene glycol is used in the alkali reduction mixture, the alkali reduction of the air suede fabric is not sufficient. Although the warp breaking strength is increased compared with Example 2, the color fastness of Comparative Examples 1 and 5 is not strong and the color difference between the upper and lower surfaces of the air suede fabric is large.
[0137] Comparative Example 3 and Comparative Example 4 and Example 2, combined with Tables 6-7, can be seen that
[0138] Because the concentration of sodium hydroxide in the alkali reduction mixture is relatively high, the alkali reduction of the fibers of the air suede fabric is uneven and the damage is relatively large, resulting in a decrease in the warp breaking strength of the air suede fabric.
[0139] Compared with Example 4, Example 3 uses a quaternary ammonium salt catalyst to promote alkali reduction. Although the alkali reduction time of Example 4 is relatively shortened compared with that of Example 3, the warp breaking strength of the air suede fabric is significantly reduced.
Claims
1. A processing technology for air layer suede fabric, It is characterized in that The steps include: S1 grey cloth → S2 pre-shrinkage → S3 flattening → S4 alkali reduction → S5 sanding → S6 dyeing → S7 dehydration and opening → S8 shaping → S9 brushing → S10 inspection and curling; The fabric obtained from the grey cloth in step S1 comprises an upper surface layer and a lower surface layer, wherein the upper surface layer is a sea-island fiber layer, and the lower surface layer is obtained by weaving low-elastic polyester fiber and spandex fiber; The alkali reduction step S4 is to treat the grey cloth with an alkali reduction mixed solution, wherein the alkali reduction mixed solution includes a quaternary ammonium salt catalyst, sodium hydroxide and water, wherein the concentration of the quaternary ammonium salt catalyst is 1-1.5 g / L, the concentration of the sodium hydroxide is 1-7 g / L, the alkali reduction time is 40-90 min, and the alkali reduction temperature is 100-110° C.; The dyeing raw materials used in step S6 include: 1.5-2.5 g / L of disperse dye, 0.3-0.8 g / L of dispersant, 1.0-2.0 g / L of leveling agent, 0.8-1.2 g / L of acetic acid, and 0.1-0.3 g / L of chitosan quaternary ammonium salt; The dyeing material in step S6 further includes carboxymethyl cellulose; the molar ratio of chitosan quaternary ammonium salt to carboxymethyl cellulose in the dyeing material in step S6 is (0.6-1):1; The dispersant includes a mixture of an amphoteric surfactant and a nonionic surfactant, and the molar ratio of the mixture of the amphoteric surfactant and the nonionic surfactant is (0.3-0.5):
1.
2. The processing technology of the air layer suede fabric according to claim 1, It is characterized in that During the alkali reduction treatment, the concentration of sodium hydroxide is 2-5 g / L, and the alkali reduction time is 50-75 min.
3. The processing technology of the air layer suede fabric according to claim 1, It is characterized in that After S4 alkali reduction, the grey cloth after alkali reduction is left to stand for 3-7 hours and then subjected to sanding treatment.
4. The processing technology of the air layer suede fabric according to claim 1, It is characterized in that The alkali-reduced mixed solution also includes aliphatic polyols, and the concentration of the aliphatic polyols is 3-5 g / L.
5. The processing technology of the air layer suede fabric according to claim 1, It is characterized in that In the dyeing step S6, the addition order of carboxymethyl cellulose takes precedence over chitosan quaternary ammonium salt, and the addition order of chitosan quaternary ammonium salt takes precedence over dispersant.
6. An air layer suede fabric, It is characterized in that The grey fabric is obtained by weaving the following raw materials and then processed by the air layer suede fabric processing process described in any one of claims 1 to 5: 35-45 parts of sea-island fiber; 47-57 parts of low-elastic polyester fiber; 6-10 parts of spandex fiber; The grey cloth comprises an upper surface layer and a lower surface layer, wherein the upper surface layer is a sea-island fiber layer, and the low-elastic polyester fiber and spandex fiber are woven to obtain the lower surface layer.
Citation Information
Patent Citations
Method for preparing suedette elastic fabric
CN105178002A
Preparing method of chamois-imitation fabric
CN109868664A
Migration inhibitor for dyeing
JP1987177287A