Polycrystalline silicon structure and preparation method thereof

By depositing multi-layer polysilicon structures in TOPCon solar cells and adjusting the deposition rate and density gradient, the problem of film explosion is solved, the uniformity and density of the film are improved, the hydrogen release phenomenon is reduced, and a convenient solution is achieved to avoid Increased cost and process complexity.

CN116314364BActive Publication Date: 2024-10-15TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310409050.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-15
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

TOPCon solar cells have a film explosion problem during the preparation process, which causes the film to easily explode and affects device performance. Existing methods require increased chemical costs or process complexity, making it difficult to effectively solve it.

Method used

By depositing a multi-layer polysilicon structure on a silicon substrate, the deposition rate and density gradient are adjusted layer by layer. The layers close to the substrate are denser and gradually loosen, reducing interface stress and hydrogen release, and reducing film bursting.

Benefits of technology

It significantly reduces the problem of membrane explosion, improves the uniformity and density of the membrane, reduces hydrogen overflow in the subsequent preparation process, avoids cost increase and process complexity, and achieves a convenient solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116314364B_ABST
    Figure CN116314364B_ABST
Patent Text Reader

Abstract

The present invention discloses a polysilicon structure and a preparation method thereof. The polysilicon structure comprises: a silicon substrate, a tunneling oxide layer, a first polysilicon layer and a second polysilicon layer, wherein the tunneling oxide layer is arranged on the silicon substrate, the first polysilicon layer is arranged on the tunneling oxide layer, the second polysilicon layer is arranged on the first polysilicon layer, and wherein the density of the second polysilicon layer is less than the density of the first polysilicon layer. The polysilicon structure and the preparation method thereof of the present invention do not need to increase the cost of other chemicals, have a large process adjustable space, are highly convenient, and can solve the problem of film explosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solar cell manufacturing, and in particular to a polycrystalline silicon structure and a preparation method thereof. Background Art

[0002] With the rapid development of photovoltaic technology, the conversion efficiency of crystalline silicon solar cells has been increasing year by year. TOPCon cells, short for tunneling oxide passivation cells, also called i-TOPCon cells, are a type of crystalline silicon solar cells. Compared with other types of cells, TOPCon cells can increase the open circuit voltage and fill factor of the cells, greatly improving the conversion rate of photovoltaics, and are therefore very popular.

[0003] In the preparation process of TOPCon cells, the current mainstream is to choose LPCVD to prepare the tunneling oxide layer and Poly (polycrystalline material) layer, and then dope the back side by diffusion. However, LPCVD itself has problems such as low poly-Si deposition rate, difficulty in in-situ doping, and damage to the quartz furnace and quartz carrier wrapping. In order to reduce costs and simplify the process, more research has turned to plasma enhanced chemical vapor deposition (PECVD) for one-step preparation of the tunneling layer and n+-poly-si, and then annealing and crystallization to complete the back structure. This preparation method has a fast deposition rate and low deposition temperature, and can directly perform in-situ doping, which simplifies many processes and achieves significant cost reduction. However, the amorphous silicon film deposited by PECVD is susceptible to poor physical contact, and bubbling usually occurs during the subsequent annealing process, causing the polysilicon film to easily explode (explode the film), resulting in a significant decrease in device performance.

[0004] There are many reasons for film explosion, including but not limited to: insufficient drying of the incoming material surface, water marks on the surface leading to film explosion, uneven or unstable temperature during the preparation process leading to film explosion, too fast deposition speed leading to the inability to release H in silane and overflowing in the subsequent preparation process leading to film explosion, etc. A large amount of evidence shows that the accumulation of interfacial stress and the rapid release of hydrogen during the crystallization process are the causes of bubbles and film explosion.

[0005] At present, some existing methods improve the film bursting by improving the flow direction of process gas and increasing the deposition temperature. In addition, there are also methods to in-situ dope carbon into polysilicon films to solve the problems of blistering and film bursting during high-temperature annealing. However, these methods either require more chemical costs, or the process has limited adjustable space, or the process is relatively complicated. Summary of the invention

[0006] In order to solve the problems existing in the existing TOPCon solar cells, the present invention provides a polysilicon structure of a solar cell and a preparation method thereof, which does not require increasing the cost of other chemicals, has a large process adjustable space, is highly convenient, and can solve the problem of film explosion.

[0007] According to one aspect of the present invention, a polysilicon structure is provided, wherein the polysilicon

[0008] The structure includes:

[0009] silicon substrate, tunnel oxide layer, first polysilicon layer and second polysilicon layer,

[0010] The tunneling oxide layer is disposed on the silicon substrate, the first polysilicon layer is disposed on the tunneling oxide layer, the second polysilicon layer is disposed on the first polysilicon layer, and

[0011] The density of the second polysilicon layer is less than the density of the first polysilicon layer.

[0012] Optionally, the density of the first polysilicon layer is 2.23-2.26 g / cm 3 The density of the second polysilicon layer is 2.20-2.23 g / cm 3 .

[0013] Optionally, the polysilicon structure further includes a third polysilicon layer, wherein the third polysilicon layer is disposed on the second polysilicon layer, and a density of the third polysilicon layer is less than a density of the second polysilicon layer.

[0014] Optionally, the density of the third polysilicon layer is 2.08-2.10 g / cm 3 .

[0015] Optionally, the polysilicon structure further includes a fourth polysilicon layer..., an Nth polysilicon layer, and an N+1th polysilicon layer, wherein N is a positive integer and N≥5, and the density of the N+1th polysilicon layer is less than the density of the Nth polysilicon layer.

[0016] The overall density of the polysilicon layer can range from 2.097-2.26 g / cm 3 The density of the polysilicon layer close to the tunnel layer is the highest, close to 2.26g / cm 3 The density of the polysilicon layer far away from the tunneling layer (outermost layer) is the lowest, which can be close to 2.097g / cm 3 .

[0017] Optionally, the polysilicon structure further includes an oxide layer, and the oxide layer is disposed on the N+1th polysilicon layer.

[0018] According to another aspect of the present invention, a method for preparing a polysilicon structure is provided, wherein the polysilicon structure comprises a silicon substrate, a tunneling oxide layer, a first polysilicon layer and a second polysilicon layer, and the preparation method comprises the following steps:

[0019] depositing a tunnel oxide layer on a silicon substrate;

[0020] depositing a first polysilicon layer on the tunnel oxide layer at a first deposition rate; and

[0021] depositing a second polysilicon layer on the first polysilicon layer at a second deposition rate higher than the first deposition rate,

[0022] The density of the second polysilicon layer is less than the density of the first polysilicon layer.

[0023] Optionally,

[0024] The preparation method further comprises:

[0025] depositing an Nth polysilicon layer on the second polysilicon layer at an Nth deposition rate higher than the second deposition rate,

[0026] Optionally, depositing an N+1th polysilicon layer on the Nth polysilicon layer at an N+1th deposition rate higher than the Nth deposition rate;

[0027] Optionally, an oxide layer is deposited on the N+1th polysilicon layer,

[0028] Wherein, N is a positive integer and N≥3, and the density of the N+1th polysilicon layer is less than the density of the Nth polysilicon layer.

[0029] Optionally, the first deposition rate is 3-6 nm / min; the second deposition rate is 6-9 nm / min; and the Nth deposition rate is 9-20 nm / min.

[0030] Optionally, the rate of depositing the polysilicon layer is adjusted by adjusting one or more of the following parameters:

[0031] Duty cycle, furnace tube reaction pressure, ventilation volume, PECVD machine microwave power, and deposition temperature.

[0032] Compared with the prior art, the present invention significantly improves the film explosion by arranging multiple layers of polysilicon on the substrate, so that the density of the outer layer is looser than that of the inner layer. The preparation method of the present invention matches different deposition rates according to a certain thickness ratio when depositing polysilicon; the deposition rate of a layer close to the substrate is slow, which can ensure the uniformity and density of the film thickness, and at the same time reduce the interfacial stress between the tunnel layer and the polysilicon layer, fully saturate the hanging hydrogen bonds, and reduce the phenomenon of H overflow in the subsequent preparation process; the deposition rate is gradually increased according to a certain gradient, and the difference in polysilicon layers prepared at different rates is reduced, so that the obtained polysilicon layer shows a dense structure when close to the silicon substrate, and then gradually loosens the gradient performance, thereby significantly reducing the film explosion problem. The polysilicon structure prepared by the preparation method of the present invention does not need to increase the cost of other chemicals, has a large process adjustable space, and is very convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to explain the present invention more clearly, the following is a brief introduction to the drawings required for the description of the technical solution. The drawings are incorporated into the specification and constitute a part of the specification, showing embodiments consistent with the present invention, and together with the specification, are used to explain the principles of the present invention. In the drawings:

[0034] Figure 1 FIG. 4 is a cross-sectional view of a polysilicon structure according to an embodiment of the present invention.

[0035] Figure 2 The figure is a flow chart of a method for preparing a polysilicon structure according to an embodiment of the present invention. DETAILED DESCRIPTION

[0036] In order to enable those skilled in the art to better understand the technical solution of the present invention, the polysilicon structure and the preparation method thereof provided by the present invention are described in detail below with reference to the accompanying drawings.

[0037] In the description of the present invention, it should be noted that the orientations or positional relationships indicated by terms such as “top”, “bottom”, “up”, “down”, “left”, “right”, “inside” and “outside” are based on the orientations or positional relationships shown in the accompanying drawings, or are the orientations or positional relationships in which the products are usually placed when in use. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0038] Furthermore, the terms “first”, “second”, etc. are merely used for distinguishing descriptions and are not to be understood as indicating or implying relative importance or order.

[0039] In addition, it should be noted that, unless there is any conflict, the features in the embodiments of the present invention may be arbitrarily combined with each other.

[0040] An embodiment of the present invention provides a polysilicon structure, referring to Figure 1 , the polysilicon structure may include: a silicon substrate 1, a tunneling oxide layer 2, a first polysilicon layer 3 and a second polysilicon layer 4. The tunneling oxide layer 2 may be disposed on the silicon substrate 1, the first polysilicon layer 3 may be disposed on the tunneling oxide layer 2, and the second polysilicon layer 4 may be disposed on the first polysilicon layer 3, wherein the density of the second polysilicon layer 4 may be less than the density of the first polysilicon layer 3. A boron-containing layer and / or an oxide layer may be disposed on the side of the silicon substrate 1 opposite to the tunneling oxide layer 2. The silicon substrate may be doped with one or more of phosphorus, arsenic and antimony.

[0041] The film explosion phenomenon generally occurs between the tunneling layer and the polysilicon layer. The polysilicon structure of the present invention has a higher density in the first polysilicon layer close to the silicon substrate, which reduces the interface stress mismatch between the tunneling oxide layer and the first polysilicon layer. The density of the second polysilicon layer deposited on the first polysilicon layer is slightly reduced, which reduces the difference between the polysilicon layers and makes the polysilicon layer present a gradient structure from dense to loose, thereby solving the film explosion problem.

[0042] In one embodiment, the density of the first polysilicon layer 3 may be 2.23-2.26 g / cm 3 , for example, 2.235 g / cm 3 , 2.24g / cm 3 , 2.245g / cm 3 , 2.25g / cm 3 , or 2.258g / cm 3 The density of the second polysilicon layer 4 can be 2.20-2.23 g / cm 3 , for example, 2.204 g / cm 3 , 2.21g / cm 3 , 2.215g / cm 3 , 2.22g / cm 3 , or 2.226g / cm 3 The density gradient setting makes the interface stress between the tunnel oxide layer and the first polysilicon layer, and between the first polysilicon layer and the second polysilicon layer in the obtained polysilicon structure match, which can significantly reduce the film explosion phenomenon.

[0043] In one embodiment, the polysilicon structure may further include a third polysilicon layer 5 (i.e., an Nth polysilicon layer, where N is a positive integer and N≥3), the third polysilicon layer 5 may be disposed on the second polysilicon layer 4, and the density of the third polysilicon layer 5 may be less than the density of the second polysilicon layer 4. Such a density setting of the polysilicon layer reduces the difference between adjacent layers and reduces the stress mismatch between layers, thereby significantly reducing the film explosion phenomenon.

[0044] In one embodiment, in order to achieve optimal stress matching between the third polysilicon layer 5 and the second polysilicon layer 4, the density of the third polysilicon layer 5 may be 2.08-2.10 g / cm 3 , for example, 2.086 g / cm 3 , 2.09g / cm 3 , 2.095g / cm 3 , or 2.098g / cm 3 wait.

[0045] In one embodiment, the polysilicon structure further includes an N+1 polysilicon layer, an N+2 polysilicon layer, an N+3 polysilicon layer, and the density of the N+2 polysilicon layer is less than the density of the N+1 polysilicon layer. In this way, the density of the polysilicon layer farther from the silicon substrate is smaller, so that the polysilicon layer presents a gradient structure with a density gradually decreasing from high to low, thereby solving the film explosion problem.

[0046] In one embodiment, according to application requirements, the polysilicon structure may generally further include an oxide layer 6. The oxide layer 6 may be disposed on the Nth polysilicon layer (i.e., the third polysilicon layer 5), i.e., on the outermost polysilicon layer, to prevent oxidation of the battery during use, thereby extending the battery life.

[0047] refer to Figure 2 The present invention also provides a method for preparing the polycrystalline silicon structure of the present invention, comprising the following steps:

[0048] S1: depositing a tunnel oxide layer 2 on a silicon substrate 1 .

[0049] The tunneling oxide layer 2 is usually an ultra-thin silicon dioxide layer, which uses the quantum tunneling effect to allow electrons to pass smoothly and prevent the recombination of holes. The tunneling oxide layer is deposited by the PECVD process, and the deposition temperature and other conditions used can adopt the conditions commonly used in the prior art. PECVD uses microwaves or radio frequencies to ionize the gas containing the atoms of the film components to form plasma locally. The plasma is very chemically active and easily reacts, thereby depositing the desired film on the silicon substrate.

[0050] S2: depositing a first polysilicon layer 3 on the tunnel oxide layer 2 at a first deposition rate.

[0051] In one embodiment, the first deposition rate may be, for example, 3-6 nm / min, such as 3.5 nm / min, 4.1 nm / min, 4.6 nm / min, 5 nm / min, 5.5 nm / min, etc. The density of the deposited first polysilicon layer 3 is close to about 97% of the density of the single crystal silicon layer. Meanwhile, the high density and uniformity can greatly reduce the occurrence of film explosion, and reduce the probability of interface stress and H overflow.

[0052] S3: depositing a second polysilicon layer 4 on the first polysilicon layer 3 at a second deposition rate.

[0053] In one embodiment, the second deposition rate is greater than the first deposition rate. The second deposition rate may be, for example, 6-9 nm / min, such as 6.3 nm / min, 6.9 nm / min, 7.4 nm / min, 7.9 nm / min, 8.3 nm / min, 8.8 nm / min, etc. The density of the second polysilicon layer may be less than the density of the first polysilicon layer. The density of the first polysilicon layer and the density of the second polysilicon layer may be in the range as described above.

[0054] In one embodiment, the above method may further include the steps of:

[0055] S4: depositing a third polysilicon layer 5 (ie, an Nth polysilicon layer, where N is a positive integer and N≥3) on the second polysilicon layer 4 at a third deposition rate.

[0056] In one embodiment, the third deposition rate (ie, the Nth deposition rate) is greater than the second deposition rate. The third deposition rate may be, for example, 9-12 nm / min, such as 9.5 nm / min, 10.2 nm / min, 10.9 nm / min, 11.3 nm / min, 11.8 nm / min, etc.

[0057] In one embodiment, the above method may further include the steps of:

[0058] S5 : depositing a fourth polysilicon layer (ie, the N+1th polysilicon layer) on the third polysilicon layer 5 at a fourth deposition rate (ie, the N+1th deposition rate).

[0059] In one embodiment, the fourth deposition rate is greater than the third deposition rate. The fourth deposition rate may be, for example, 12-20 nm / min, such as 12.5 nm / min, 13 nm / min, 15 nm / min, 17 nm / min, 18.5 nm / min, etc.

[0060] The deposition rates of the above-mentioned polysilicon layers can achieve a step-by-step change in the density of the silicon layer.

[0061] In one embodiment, the above method may further include the steps of:

[0062] S6: depositing an oxide layer on the N+1th polysilicon layer.

[0063] Similarly, the polysilicon layer is deposited by the PECVD process. The PECVD polysilicon deposition rate is fast, in-situ doping can be achieved, and the plating area is easy to remove. At the same time, the consumables only need to clean the graphite boat regularly, there is no quartz tube consumables, and no pre-plating quartz tube is required. If the common film explosion problem in PECVD can be solved, the cost of battery preparation can be greatly reduced while ensuring the efficiency and yield are the same.

[0064] The preparation method of the present invention matches different deposition rates according to a certain thickness ratio when depositing polysilicon; controls the deposition rate slowly in a layer close to the silicon substrate, thereby ensuring the uniformity and density of the film thickness, and at the same time reduces the interfacial stress between the tunnel layer and the polysilicon layer, fully saturates the hanging hydrogen bonds, and reduces the phenomenon of H overflow in the subsequent preparation process; and gradually increases the deposition rate according to a certain gradient to reduce the difference in polysilicon layers prepared at different rates. The polysilicon layer in the polysilicon structure prepared by the preparation method of the present invention presents a gradient performance in which the structure is dense when close to the silicon substrate, and then gradually becomes loose, thereby solving the problem that the polysilicon film deposited by PECVD is prone to film explosion.

[0065] The method for solving the film explosion in the present invention does not need to increase the cost of other chemicals, has a large process adjustable space, and is very convenient.

[0066] In one embodiment, the rate of depositing the polysilicon layer is adjusted by adjusting one or more of the following parameters: duty cycle, furnace tube reaction pressure, ventilation volume, PECVD machine microwave power, and deposition temperature. For example, the deposition rate can be slowed down by increasing the duty cycle, increasing the pressure, reducing the gas volume, reducing the power, or adjusting the temperature.

[0067] The present invention is further illustrated by means of specific examples below.

[0068] Example 1

[0069] Taking the growth of a Poly layer of a certain total thickness by in-situ doping as an example, after the tunnel oxide layer is prepared, first, a layer of n1 polysilicon is grown, and the deposition rate is slowed down by process adjustment (such as increasing the duty cycle, increasing the pressure, reducing the gas volume, reducing the power or adjusting the temperature), and the deposition density is 2.23-2.26g / cm 3The polysilicon layer of n2 is grown. The density of this polysilicon layer is close to that of the single crystal silicon layer. At the same time, the high density and uniformity can greatly reduce the occurrence of film explosion, reduce the probability of interface stress and H overflow; the n2 polysilicon layer is then grown. The deposition rate is faster than that of n1, and the density is looser than that of n1 layer, ranging from about 2.20-2.23g / cm 3 Similarly, the deposition rate is then gradually increased according to a certain gradient to prepare a multi-layer (n ≥ 3) polysilicon layer, and the density of the outermost polysilicon layer is about 2.08-2.10 g / cm 3 After the polysilicon is prepared, an oxide layer is prepared on the outermost layer as a mask.

[0070] The polysilicon structure obtained in the above-mentioned embodiment 1 is mainly characterized by gradient preparation of the density and compactness of the polysilicon layer, and a polysilicon layer close to the silicon substrate is very dense and gradually becomes loose poly film layer structure, so as to solve the film explosion problem occurring during PECVD deposition.

[0071] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A polycrystalline silicon structure, characterized in that: The polysilicon structure comprises: silicon substrate, tunnel oxide layer, first polysilicon layer and second polysilicon layer, The tunneling oxide layer is disposed on the silicon substrate, the first polysilicon layer is disposed on the tunneling oxide layer, the second polysilicon layer is disposed on the first polysilicon layer, and wherein the density of the second polysilicon layer is less than the density of the first polysilicon layer, The density of the first polysilicon layer is 2.23-2.26 g / cm 3 The density of the second polysilicon layer is 2.20-2.23 g / cm 3 .

2. The polysilicon structure according to claim 1, characterized in that: The polysilicon structure further includes a third polysilicon layer, which is disposed on the second polysilicon layer, and has a density less than that of the second polysilicon layer.

3. The polysilicon structure according to claim 2, characterized in that: The density of the third polysilicon layer is 2.08-2.10 g / cm 3 .

4. The polysilicon structure according to claim 2, characterized in that: The polysilicon structure further includes a fourth polysilicon layer, ..., an Nth polysilicon layer, and an N+1th polysilicon layer, wherein N is a positive integer and N≥5, and the density of the N+1th polysilicon layer is less than the density of the Nth polysilicon layer.

5. The polysilicon structure according to claim 4, characterized in that: The polysilicon structure further includes an oxide layer, and the oxide layer is disposed on the N+1th polysilicon layer.

6. A method for preparing a polysilicon structure, wherein the polysilicon structure comprises a silicon substrate, a tunneling oxide layer, a first polysilicon layer and a second polysilicon layer, characterized in that: The preparation method comprises the following steps: depositing a tunnel oxide layer on a silicon substrate; depositing a first polysilicon layer on the tunnel oxide layer at a first deposition rate; and depositing a second polysilicon layer on the first polysilicon layer at a second deposition rate higher than the first deposition rate, wherein the density of the second polysilicon layer is less than the density of the first polysilicon layer, The density of the first polysilicon layer is 2.23-2.26 g / cm 3 The density of the second polysilicon layer is 2.20-2.23 g / cm 3 .

7. The preparation method according to claim 6, characterized in that: The preparation method further comprises: depositing an Nth polysilicon layer on the second polysilicon layer at an Nth deposition rate higher than the second deposition rate, Wherein, N is a positive integer and N≥3.

8. The preparation method according to claim 7, characterized in that: The preparation method further comprises: depositing an N+1th polysilicon layer on the Nth polysilicon layer at an N+1th deposition rate higher than the Nth deposition rate, The density of the N+1th polysilicon layer is less than the density of the Nth polysilicon layer.

9. The preparation method according to claim 8, characterized in that: The preparation method further comprises: An oxide layer is deposited on the N+1th polysilicon layer.

10. The preparation method according to claim 7, characterized in that: The first deposition rate is 3-6 nm / min; the second deposition rate is 6-9 nm / min; and the Nth deposition rate is 9-20 nm / min.

11. The preparation method according to any one of claims 6 to 10, characterized in that: The rate of depositing the polysilicon layer is adjusted by adjusting one or more of the following parameters: Duty cycle, furnace tube reaction pressure, ventilation volume, PECVD machine microwave power, and deposition temperature.